Al6061 NI results NIST Project Ali Khosravani Jordan Weaver

Upload: alikhosravani

Post on 27-Jul-2015

78 views

Category:

Engineering


0 download

TRANSCRIPT

Page 1: Al6061 Nanoindentation results

Al6061 NI resultsNIST Project

Ali KhosravaniJordan Weaver

Page 2: Al6061 Nanoindentation results
Page 3: Al6061 Nanoindentation results

4

5

6

7

8

x 10-3

50

55

60

65

70-0.1

0

0.1

0.2

0.3

0.4

0.5

0.6

Fit4 Average Abs ResidualEeff

h-c

han

ge

Fit

4 M

ax A

bs

Res

idu

al

0.014

0.015

0.016

0.017

0.018

0.019

0.02

0.021

0.022

0.023

Aged at 400F for 2hrs_ 100micron tip_001

Page 4: Al6061 Nanoindentation results

AR_ 100micron tip_ test 001

65 70 75 800

20

40

Modulus [GPa]

0.96 0.98 1 1.020

20

40

R2

40 60 80 1000

20

40

Modulus Length [#points]-0.7 -0.6 -0.5 -0.4 -0.30

20

40

Hr [nm]

0.009 0.01 0.011 0.012 0.0130

50

Fit1 Avg.Abs.Res.0.02 0.03 0.04 0.05 0.060

20

40

Fit1 Max.Abs.Res.0.1 0.11 0.12 0.130

20

40

Fit2 Avg.Abs.Res.0.25 0.3 0.35 0.4 0.450

20

40

Fit2 Max.Abs.Res.

0.5 0.6 0.7 0.8 0.90

50

h change [nm/nm]0.4 0.5 0.6 0.7

0

20

40

P change [mN/mN]6 6.5 7 7.5

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.018 0.02 0.022 0.0240

20

40

Fit4 Max.Abs.Res.

0.2 0.21 0.22 0.230

20

40

P* [mN]

18.5 19 19.50

20

40

h* [nm]

0 1 2 3

x 10-3

0

10

20

dP [mN]-0.2 -0.1 0 0.1 0.20

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 5: Al6061 Nanoindentation results

AR_ 100micron tip_ test 001Estat = mean: 74.0953 median: 74.5196 stdev: 1.4504 min: 70.4381 max: 75.9712

Ystat = mean: 0.5090 median: 0.5134 stdev: 0.0169 min: 0.4678 max: 0.5321

Hstat = mean: 26.4590 median: 26.6196 stdev: 0.5423 min: 25.0907 max: 27.1902

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=70.4792; Bunge=0, 0, 0; Strength=0.50739; Hardening=26.4099

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 5 10 15

x 104

-2.5

-2

-1.5

-1

-0.5

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.2 0.4 0.6 0.8-2

0

2

4

6

8

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 6: Al6061 Nanoindentation results

AR_ 100micron tip_ test 003

66 68 70 72 74 760

20

40

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

100

200

R2

0 50 100 1500

50

100

Modulus Length [#points]-2 -1.5 -1 -0.5 0

0

50

100

Hr [nm]

0 0.01 0.02 0.03 0.040

50

100

Fit1 Avg.Abs.Res.0 0.05 0.1 0.15 0.2

0

100

200

Fit1 Max.Abs.Res.0 0.1 0.2 0.3 0.4

0

50

100

Fit2 Avg.Abs.Res.0 0.5 1 1.5

0

50

100

Fit2 Max.Abs.Res.

0 0.2 0.4 0.6 0.80

50

100

h change [nm/nm]0.1 0.2 0.3 0.4 0.5 0.60

50

100

P change [mN/mN]4 5 6 7 8

x 10-3

0

50

100

Fit4 Avg.Abs.Res.0.012 0.014 0.016 0.018 0.02 0.0220

50

100

Fit4 Max.Abs.Res.

0.2 0.4 0.6 0.8 10

50

100

P* [mN]

14 16 18 20 22 240

50

100

h* [nm]

0 1 2 3 4

x 10-3

0

20

40

dP [mN]-0.6 -0.4 -0.2 0 0.2 0.40

50

100

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 7: Al6061 Nanoindentation results

AR_ 100micron tip_ test 003Estat = mean: 72.8881 median: 72.7568 stdev: 1.7132 min: 70.0032 max: 75.9966

Ystat = mean: 0.5726 median: 0.5718 stdev: 0.0247 min: 0.4797 max: 0.6337

Hstat = mean: 25.9397 median: 25.8888 stdev: 0.6667 min: 24.6468 max: 27.2296

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

1.2

1.4

1.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4139; Bunge=0, 0, 0; Strength=0.58068; Hardening=25.8184

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2 2.5

x 105

-6

-5

-4

-3

-2

-1

0

1x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 2-5

0

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 8: Al6061 Nanoindentation results

AR_ 100micron tip_ test 004

65 70 75 800

10

20

Modulus [GPa]

0.99 0.995 1 1.0050

20

40

R2

110 120 130 140 1500

20

40

Modulus Length [#points]-1.4 -1.2 -1 -0.8 -0.60

10

20

Hr [nm]

0.008 0.01 0.012 0.0140

20

40

Fit1 Avg.Abs.Res.0.02 0.04 0.06 0.080

20

40

Fit1 Max.Abs.Res.0.2 0.25 0.3 0.35

0

20

40

Fit2 Avg.Abs.Res.0.5 1 1.50

20

40

Fit2 Max.Abs.Res.

-0.1 0 0.1 0.2 0.30

20

40

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

10

20

P change [mN/mN]3.8 4 4.2 4.4 4.6

x 10-3

0

10

20

Fit4 Avg.Abs.Res.0.011 0.012 0.013 0.014 0.0150

50

Fit4 Max.Abs.Res.

0.35 0.4 0.45 0.50

20

40

P* [mN]

22 22.5 23 23.5 240

20

40

h* [nm]

0 1 2 3 4

x 10-3

0

10

20

dP [mN]-0.2 0 0.2 0.4 0.60

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 9: Al6061 Nanoindentation results

AR_ 100micron tip_ test 004Estat = mean: 72.9264 median: 72.7957 stdev: 1.7328 min: 70.0236 max: 75.9430

Ystat = mean: 0.5620 median: 0.5603 stdev: 0.0253 min: 0.5206 max: 0.6081

Hstat = mean: 25.3096 median: 25.2949 stdev: 0.6958 min: 24.1726 max: 26.5177

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.3459; Bunge=0, 0, 0; Strength=0.55924; Hardening=25.3294

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-6

-5

-4

-3

-2

-1

0

1x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 20

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 10: Al6061 Nanoindentation results

AR_ 100micron tip_ test 005

66 68 70 72 74 760

10

20

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

50

100

R2

20 40 60 80 100 1200

20

40

Modulus Length [#points]-0.7 -0.6 -0.5 -0.4 -0.30

50

Hr [nm]

4 6 8 10

x 10-3

0

50

Fit1 Avg.Abs.Res.0.01 0.02 0.03 0.04 0.050

50

100

Fit1 Max.Abs.Res.0.08 0.1 0.12 0.14 0.160

50

100

Fit2 Avg.Abs.Res.0.25 0.3 0.35 0.4 0.450

100

200

Fit2 Max.Abs.Res.

0 0.2 0.4 0.6 0.80

20

40

h change [nm/nm]0 0.1 0.2 0.3 0.4 0.5

0

20

40

P change [mN/mN]4 5 6 7 8

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.016 0.018 0.02 0.0220

20

40

Fit4 Max.Abs.Res.

0.25 0.3 0.35 0.4 0.450

50

P* [mN]

18.5 19 19.5 20 20.5 210

50

100

h* [nm]

0 1 2 3 4

x 10-3

0

10

20

dP [mN]-0.4 -0.2 0 0.2 0.40

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 11: Al6061 Nanoindentation results

AR_ 100micron tip_ test 005Estat = mean: 72.9738 median: 73.0464 stdev: 1.7727 min: 70.0284 max: 75.9751

Ystat = mean: 0.5677 median: 0.5668 stdev: 0.0264 min: 0.5105 max: 0.6133

Hstat = mean: 24.2864 median: 24.3030 stdev: 0.6177 min: 23.2218 max: 25.3615

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4103; Bunge=0, 0, 0; Strength=0.56771; Hardening=24.2611

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 5 10 15

x 104

-3

-2.5

-2

-1.5

-1

-0.5

0

0.5x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1-2

0

2

4

6

8

10

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 12: Al6061 Nanoindentation results

AR_ 100micron tip_ test 006

65 70 75 800

5

10

Modulus [GPa]

0.94 0.96 0.98 10

10

20

R2

20 30 40 50 600

5

10

Modulus Length [#points]-0.6 -0.5 -0.4 -0.3 -0.20

10

20

Hr [nm]

4 5 6 7

x 10-3

0

10

20

Fit1 Avg.Abs.Res.0.005 0.01 0.015 0.02 0.0250

10

20

Fit1 Max.Abs.Res.0.08 0.1 0.12 0.140

10

20

Fit2 Avg.Abs.Res.0.2 0.3 0.4 0.50

5

10

Fit2 Max.Abs.Res.

-0.5 0 0.5 10

10

20

h change [nm/nm]0 0.2 0.4 0.6 0.8

0

10

20

P change [mN/mN]4 5 6 7

x 10-3

0

10

20

Fit4 Avg.Abs.Res.0.01 0.015 0.020

5

10

Fit4 Max.Abs.Res.

0.2 0.25 0.3 0.35 0.40

10

20

P* [mN]

10 11 12 13 140

10

20

h* [nm]

0 1 2 3 4

x 10-3

0

5

10

dP [mN]-0.2 0 0.2 0.4 0.60

10

20

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 13: Al6061 Nanoindentation results

AR_ 100micron tip_ test 006Estat = mean: 72.7770 median: 72.6317 stdev: 1.6269 min: 70.0297 max: 75.9841

Ystat = mean: 1.3887 median: 0.5726 stdev: 0.8684 min: 0.4794 max: 2.3706

Hstat = mean: -20.5747 median: 24.3717 stdev: 46.3225 min: -68.8533 max: 25.6614

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

1.2

1.4

1.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.1032; Bunge=0, 0, 0; Strength=0.55979; Hardening=25.303

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 5 10 15

x 104

-2

-1.5

-1

-0.5

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.2 0.4 0.6 0.8-2

0

2

4

6

8

10

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 14: Al6061 Nanoindentation results

AR_ 100micron tip_ test 007

65 70 75 800

10

20

Modulus [GPa]

0.985 0.99 0.995 1 1.0050

20

40

R2

90 100 110 1200

10

20

Modulus Length [#points]-0.9 -0.8 -0.7 -0.6 -0.50

10

20

Hr [nm]

0.01 0.015 0.020

10

20

Fit1 Avg.Abs.Res.0.03 0.04 0.05 0.060

10

20

Fit1 Max.Abs.Res.0.2 0.25 0.3 0.35

0

10

20

Fit2 Avg.Abs.Res.0 0.5 1 1.5

0

10

20

Fit2 Max.Abs.Res.

0 0.1 0.2 0.3 0.40

10

20

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

10

20

P change [mN/mN]5.5 6 6.5 7

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.016 0.018 0.02 0.0220

10

20

Fit4 Max.Abs.Res.

0.48 0.5 0.52 0.54 0.560

10

20

P* [mN]

18 18.5 19 19.50

10

20

h* [nm]

0 2 4 6

x 10-3

0

10

20

dP [mN]-0.5 0 0.50

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 15: Al6061 Nanoindentation results

AR_ 100micron tip_ test 007Estat = mean: 72.2464 median: 71.9764 stdev: 1.6662 min: 70.0129 max: 75.9662

Ystat = mean: 0.5074 median: 0.5047 stdev: 0.0193 min: 0.4798 max: 0.5531

Hstat = mean: 25.7443 median: 25.7191 stdev: 0.7086 min: 24.5450 max: 27.1741

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.7734; Bunge=0, 0, 0; Strength=0.50939; Hardening=25.8316

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-5

-4

-3

-2

-1

0

1x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 20

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 16: Al6061 Nanoindentation results

AR_ 100micron tip_ test 009

66 68 70 72 74 760

10

20

Modulus [GPa]

0.96 0.97 0.98 0.99 1 1.010

20

40

R2

40 60 80 100 1200

10

20

Modulus Length [#points]-0.8 -0.6 -0.4 -0.2 00

10

20

Hr [nm]

5 6 7 8 9 10

x 10-3

0

10

20

Fit1 Avg.Abs.Res.0.01 0.02 0.03 0.04 0.050

50

Fit1 Max.Abs.Res.0.11 0.12 0.13 0.14 0.15 0.160

10

20

Fit2 Avg.Abs.Res.0.2 0.4 0.6 0.8 10

10

20

Fit2 Max.Abs.Res.

-0.05 0 0.05 0.1 0.15 0.20

5

10

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

5

10

P change [mN/mN]4 5 6 7

x 10-3

0

10

20

Fit4 Avg.Abs.Res.0.014 0.016 0.018 0.02 0.022 0.0240

5

10

Fit4 Max.Abs.Res.

0.25 0.3 0.35 0.4 0.450

20

40

P* [mN]

14 15 16 17 180

20

40

h* [nm]

0 1 2 3 4

x 10-3

0

5

10

dP [mN]-0.4 -0.2 0 0.2 0.40

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 17: Al6061 Nanoindentation results

AR_ 100micron tip_ test 009Estat = mean: 72.3650 median: 72.3985 stdev: 1.6707 min: 70.0855 max: 75.9545

Ystat = mean: 0.6027 median: 0.6021 stdev: 0.0314 min: 0.5364 max: 0.6666

Hstat = mean: 25.0466 median: 25.0440 stdev: 0.5939 min: 24.1868 max: 26.2760

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.8635; Bunge=0, 0, 0; Strength=0.60705; Hardening=25.0446

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-4

-3

-2

-1

0

1x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.50

2

4

6

8

10

12

14

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 18: Al6061 Nanoindentation results

AR_ 100micron tip_ test 010

Page 19: Al6061 Nanoindentation results

AR_ 100micron tip_ test 010Estat = mean: 72.5138 median: 72.2047 stdev: 1.5804 min: 70.0063 max: 75.9970

Ystat = mean: 1.1205 median: 1.1902 stdev: 0.2391 min: 0.3946 max: 1.3185

Hstat = mean: 10.6983 median: 8.5662 stdev: 5.5002 min: 8.2477 max: 27.3548

Page 20: Al6061 Nanoindentation results

400F_ 100micron tip_ test 001

66 68 70 72 74 760

20

40

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

200

400

R2

60 80 100 1200

20

40

Modulus Length [#points]-6 -4 -2 0

0

20

40

Hr [nm]

0 0.05 0.1 0.15 0.2 0.250

50

100

Fit1 Avg.Abs.Res.0 0.2 0.4 0.6 0.8

0

50

100

Fit1 Max.Abs.Res.0 0.2 0.4 0.6 0.8 1

0

50

100

Fit2 Avg.Abs.Res.0 1 2 3 4

0

50

Fit2 Max.Abs.Res.

0 0.1 0.2 0.3 0.40

50

h change [nm/nm]0 0.1 0.2 0.3 0.4

0

50

P change [mN/mN]0.005 0.01 0.015 0.020

50

100

Fit4 Avg.Abs.Res.0.01 0.02 0.03 0.04 0.050

20

40

Fit4 Max.Abs.Res.

0 2 4 6 80

50

P* [mN]

0 20 40 600

50

h* [nm]

0 0.01 0.02 0.03 0.04 0.050

20

40

dP [mN]-1.5 -1 -0.5 0 0.5 10

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 21: Al6061 Nanoindentation results

Estat = mean: 72.7560 median: 72.6725 stdev: 1.7194 min: 70.0141 max: 75.9311

Ystat = mean: 0.5800 median: 0.5799 stdev: 0.0273 min: 0.5142 max: 0.6424

Hstat = mean: 25.7733 median: 25.7376 stdev: 0.8190 min: 23.9460 max: 27.7413

400F_ 100micron tip_ test 001

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.1823; Bunge=0, 0, 0; Strength=0.60068; Hardening=25.4006

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

-1 0 1 2 3

x 105

-15

-10

-5

0

5x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 3 40

10

20

30

40

50

P 2/3

h

Modulus Fit

Data

Elastic

0 0.02 0.04 0.06 0.08 0.10

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 22: Al6061 Nanoindentation results

400F_ 100micron tip_ test 002

66 68 70 72 74 760

20

40

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

100

200

R2

60 80 100 1200

50

Modulus Length [#points]-6 -4 -2 0

0

50

Hr [nm]

0 0.05 0.1 0.15 0.20

50

100

Fit1 Avg.Abs.Res.0 0.2 0.4 0.6 0.8

0

50

Fit1 Max.Abs.Res.0 0.2 0.4 0.6 0.8 1

0

50

100

Fit2 Avg.Abs.Res.0 1 2 3 4

0

50

Fit2 Max.Abs.Res.

0 0.1 0.2 0.3 0.4 0.50

50

h change [nm/nm]0 0.1 0.2 0.3 0.4

0

50

P change [mN/mN]0.005 0.01 0.015 0.020

50

100

Fit4 Avg.Abs.Res.0.015 0.02 0.025 0.03 0.035 0.040

20

40

Fit4 Max.Abs.Res.

0 2 4 60

20

40

P* [mN]

0 10 20 30 40 500

20

40

h* [nm]

0 0.01 0.02 0.03 0.04 0.050

20

40

dP [mN]-2 -1 0 1 2

0

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 23: Al6061 Nanoindentation results

400F_ 100micron tip_ test 002Estat = mean: 72.5480 median: 72.3265 stdev: 1.7056 min: 70.0063 max: 75.9879

Ystat = mean: 0.6048 median: 0.6052 stdev: 0.0245 min: 0.5445 max: 0.6608

Hstat = mean: 26.2425 median: 26.1201 stdev: 0.7859 min: 24.9040 max: 28.0767

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.8711; Bunge=0, 0, 0; Strength=0.61391; Hardening=25.8814

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

-1 0 1 2 3

x 105

-12

-10

-8

-6

-4

-2

0

2x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 3 40

10

20

30

40

P 2/3

h

Modulus Fit

Data

Elastic

0 0.2 0.4 0.60

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 24: Al6061 Nanoindentation results

400F_ 100micron tip_ test 003

65 70 75 800

10

20

Modulus [GPa]

0.94 0.96 0.98 10

50

100

R2

80 90 100 110 1200

20

40

Modulus Length [#points]-4 -3 -2 -1 0

0

20

40

Hr [nm]

0 0.02 0.04 0.06 0.080

20

40

Fit1 Avg.Abs.Res.0 0.1 0.2 0.3 0.4

0

20

40

Fit1 Max.Abs.Res.0 0.2 0.4 0.6 0.8

0

50

Fit2 Avg.Abs.Res.0 1 2 3

0

20

40

Fit2 Max.Abs.Res.

0 0.1 0.2 0.3 0.40

20

40

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

50

100

P change [mN/mN]0.005 0.01 0.0150

20

40

Fit4 Avg.Abs.Res.0.01 0.02 0.03 0.040

20

40

Fit4 Max.Abs.Res.

0 1 2 3 40

10

20

P* [mN]

0 10 20 30 400

20

40

h* [nm]

0 0.02 0.04 0.060

20

40

dP [mN]-0.5 0 0.5 1 1.50

10

20

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 25: Al6061 Nanoindentation results

400F_ 100micron tip_ test 003

Estat = mean: 73.0235 median: 73.0678 stdev: 1.7908 min: 70.0025 max: 75.9985

Ystat = mean: 0.5911 median: 0.5877 stdev: 0.0241 min: 0.5384 max: 0.6472

Hstat = mean: 26.7180 median: 26.7403 stdev: 0.7762 min: 25.1076 max: 28.2214

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

1.2

1.4

1.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.6973; Bunge=0, 0, 0; Strength=0.57997; Hardening=27.0297

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

-2 0 2 4

x 105

-20

-15

-10

-5

0

5x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 2 4 6-10

0

10

20

30

40

50

P 2/3

h

Modulus Fit

Data

Elastic

0 0.1 0.2 0.30

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 26: Al6061 Nanoindentation results

400F_ 100micron tip_ test 004

66 68 70 72 74 760

10

20

Modulus [GPa]

0.97 0.98 0.99 1 1.010

20

40

R2

80 90 100 110 1200

20

40

Modulus Length [#points]-3.5 -3 -2.5 -2 -1.5 -10

20

40

Hr [nm]

0.02 0.04 0.06 0.080

20

40

Fit1 Avg.Abs.Res.0.05 0.1 0.15 0.2 0.250

20

40

Fit1 Max.Abs.Res.0.2 0.3 0.4 0.5 0.6 0.70

20

40

Fit2 Avg.Abs.Res.1 1.5 2 2.5 3

0

20

40

Fit2 Max.Abs.Res.

0 0.05 0.1 0.15 0.2 0.250

20

40

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

20

40

P change [mN/mN]4 6 8 10 12

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.01 0.015 0.02 0.025 0.030

20

40

Fit4 Max.Abs.Res.

0.5 1 1.5 2 2.5 30

20

40

P* [mN]

10 15 20 25 300

20

40

h* [nm]

0 0.005 0.01 0.015 0.020

20

40

dP [mN]-0.5 0 0.5 10

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 27: Al6061 Nanoindentation results

400F_ 100micron tip_ test 004Estat = mean: 72.9889 median: 73.1361 stdev: 1.8000 min: 70.0546 max: 75.9991

Ystat = mean: 0.6103 median: 0.6072 stdev: 0.0260 min: 0.5609 max: 0.6650

Hstat = mean: 26.9273 median: 26.9275 stdev: 0.7568 min: 25.5735 max: 28.3435

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

1.2

1.4

1.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4253; Bunge=0, 0, 0; Strength=0.6109; Hardening=26.7417

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

-1 0 1 2 3

x 105

-8

-6

-4

-2

0

2x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 30

5

10

15

20

25

30

P 2/3

h

Modulus Fit

Data

Elastic

0 0.05 0.10

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 28: Al6061 Nanoindentation results

400F_ 100micron tip_ test 005

66 68 70 72 74 760

20

40

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

50

100

R2

60 80 100 1200

20

40

Modulus Length [#points]-4 -3 -2 -1 0

0

50

100

Hr [nm]

0 0.02 0.04 0.06 0.08 0.10

50

100

Fit1 Avg.Abs.Res.0 0.05 0.1 0.15 0.2 0.25

0

50

100

Fit1 Max.Abs.Res.0 0.2 0.4 0.6 0.8

0

50

100

Fit2 Avg.Abs.Res.0 1 2 3 4

0

20

40

Fit2 Max.Abs.Res.

-0.1 0 0.1 0.2 0.30

20

40

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

20

40

P change [mN/mN]4 6 8 10 12

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.01 0.015 0.02 0.0250

20

40

Fit4 Max.Abs.Res.

0 1 2 3 40

50

100

P* [mN]

0 10 20 30 400

50

100

h* [nm]

0 0.005 0.01 0.015 0.020

50

dP [mN]-0.5 0 0.5 10

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 29: Al6061 Nanoindentation results

400F_ 100micron tip_ test 005Estat = mean: 72.4187 median: 72.3209 stdev: 1.5646 min: 70.0299 max: 75.9694

Ystat = mean: 0.5981 median: 0.5954 stdev: 0.0208 min: 0.5477 max: 0.6574

Hstat =

mean: 25.8628 median: 25.7550 stdev: 0.6907 min: 24.7395 max: 27.5316

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.8299; Bunge=0, 0, 0; Strength=0.58431; Hardening=25.9528

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3

x 105

-12

-10

-8

-6

-4

-2

0

2x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 3 40

10

20

30

40

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 30: Al6061 Nanoindentation results

400F_ 100micron tip_ test 006

66 68 70 72 74 760

10

20

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

100

200

R2

60 70 80 90 100 1100

10

20

Modulus Length [#points]-4 -3 -2 -1 0

0

20

40

Hr [nm]

0 0.02 0.04 0.06 0.080

20

40

Fit1 Avg.Abs.Res.0 0.05 0.1 0.15 0.2 0.25

0

20

40

Fit1 Max.Abs.Res.0 0.2 0.4 0.6 0.8

0

50

100

Fit2 Avg.Abs.Res.0 1 2 3

0

20

40

Fit2 Max.Abs.Res.

0 0.1 0.2 0.3 0.4 0.50

50

100

h change [nm/nm]0 0.1 0.2 0.3 0.4

0

50

100

P change [mN/mN]5 6 7 8 9 10

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.015 0.02 0.025 0.030

20

40

Fit4 Max.Abs.Res.

0 1 2 3 40

20

40

P* [mN]

0 10 20 30 400

20

40

h* [nm]

0 0.005 0.01 0.015 0.020

20

40

dP [mN]-0.5 0 0.5 10

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 31: Al6061 Nanoindentation results

400F_ 100micron tip_ test 006Estat = mean: 72.5387 median: 72.3448 stdev: 1.6706 min: 70.0031 max: 75.9708

Ystat = mean: 0.6235 median: 0.6197 stdev: 0.0376 min: 0.5521 max: 0.7019

Hstat = mean: 25.2648 median: 25.1910 stdev: 0.6441 min: 24.1051 max: 26.5741

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

1.2

1.4

1.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.9125; Bunge=0, 0, 0; Strength=0.64253; Hardening=25.1394

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3

x 105

-15

-10

-5

0

5x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 3 40

10

20

30

40

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 32: Al6061 Nanoindentation results

400F_ 100micron tip_ test 007

66 68 70 72 74 760

10

20

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

20

40

R2

95 100 105 110 115 1200

10

20

Modulus Length [#points]-3 -2.5 -2 -1.5 -1

0

10

20

Hr [nm]

0.02 0.03 0.04 0.05 0.060

10

20

Fit1 Avg.Abs.Res.0.05 0.1 0.15 0.2 0.250

10

20

Fit1 Max.Abs.Res.0.35 0.4 0.45 0.5 0.55 0.6

0

10

20

Fit2 Avg.Abs.Res.1 1.5 2 2.5 3

0

10

20

Fit2 Max.Abs.Res.

-0.05 0 0.05 0.1 0.150

20

40

h change [nm/nm]0 0.02 0.04 0.06 0.08 0.1

0

20

40

P change [mN/mN]5 6 7 8 9 10

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.015 0.02 0.025 0.030

10

20

Fit4 Max.Abs.Res.

0.5 1 1.5 2 2.50

10

20

P* [mN]

10 15 20 250

10

20

h* [nm]

0 0.005 0.01 0.015 0.020

10

20

dP [mN]-0.5 0 0.5 10

10

20

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 33: Al6061 Nanoindentation results

400F_ 100micron tip_ test 007

Estat = mean: 72.5940 median: 72.4691 stdev: 1.6808 min: 70.0073 max: 75.9954

Ystat = mean: 0.6301 median: 0.6262 stdev: 0.0239 min: 0.5901 max: 0.6833

Hstat = mean: 24.2083 median: 24.1450 stdev: 0.6232 min: 23.2490 max: 25.4870

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.9381; Bunge=0, 0, 0; Strength=0.62268; Hardening=24.145

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3

x 105

-15

-10

-5

0

5x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 3 40

10

20

30

40

50

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 34: Al6061 Nanoindentation results

400F_ 100micron tip_ test 008

65 70 75 800

5

10

Modulus [GPa]

0.94 0.96 0.98 10

5

10

R2

70 75 80 85 900

5

10

Modulus Length [#points]-3 -2.5 -2 -1.5 -1

0

10

20

Hr [nm]

0.03 0.04 0.05 0.060

5

10

Fit1 Avg.Abs.Res.0.08 0.1 0.12 0.14 0.160

5

10

Fit1 Max.Abs.Res.0.35 0.4 0.45 0.5

0

5

10

Fit2 Avg.Abs.Res.1 1.5 2 2.5

0

10

20

Fit2 Max.Abs.Res.

0 0.05 0.1 0.15 0.20

10

20

h change [nm/nm]0 0.05 0.1 0.15 0.2

0

20

40

P change [mN/mN]6 8 10 12

x 10-3

0

5

10

Fit4 Avg.Abs.Res.0.018 0.02 0.022 0.024 0.0260

5

10

Fit4 Max.Abs.Res.

1.4 1.6 1.8 2 2.20

5

10

P* [mN]

16 18 20 22 240

5

10

h* [nm]

0 0.005 0.01 0.015 0.020

5

10

dP [mN]-0.5 0 0.5 10

5

10

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 35: Al6061 Nanoindentation results

400F_ 100micron tip_ test 008Estat = mean: 72.8347 median: 72.7764 stdev: 1.7629 min: 70.0515 max: 75.9819

Ystat = mean: 0.6153 median: 0.6150 stdev: 0.0243 min: 0.5745 max: 0.6635

Hstat = mean: 25.5687 median: 25.5641 stdev: 0.6504 min: 24.5436 max: 26.8152

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

1.2

1.4

1.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.3031; Bunge=0, 0, 0; Strength=0.61882; Hardening=25.6051

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

-1 0 1 2 3

x 105

-10

-8

-6

-4

-2

0

2x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 3-10

0

10

20

30

40

P 2/3

h

Modulus Fit

Data

Elastic

0 0.1 0.20

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 36: Al6061 Nanoindentation results

400F_ 100micron tip_ test 009

65 70 75 800

10

20

Modulus [GPa]

0.94 0.96 0.98 10

10

20

R2

90 100 110 1200

20

40

Modulus Length [#points]-2 -1.5 -1 -0.5

0

10

20

Hr [nm]

0.02 0.03 0.04 0.050

20

40

Fit1 Avg.Abs.Res.0.05 0.1 0.150

10

20

Fit1 Max.Abs.Res.0.35 0.4 0.45 0.5

0

10

20

Fit2 Avg.Abs.Res.1 1.5 2 2.5

0

10

20

Fit2 Max.Abs.Res.

-0.05 0 0.05 0.1 0.150

10

20

h change [nm/nm]0 0.05 0.1

0

10

20

P change [mN/mN]4 6 8 10

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.015 0.02 0.025 0.030

10

20

Fit4 Max.Abs.Res.

0.5 1 1.5 20

10

20

P* [mN]

10 15 200

10

20

h* [nm]

0 0.005 0.01 0.015 0.020

10

20

dP [mN]0.2 0.4 0.6 0.8 10

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 37: Al6061 Nanoindentation results

400F_ 100micron tip_ test 009Estat = mean: 72.7375 median: 72.5867 stdev: 1.7351 min: 70.0108 max: 75.9380

Ystat = mean: 0.5990 median: 0.5987 stdev: 0.0244 min: 0.5534 max: 0.6502

Hstat = mean: 25.0370 median: 25.0045 stdev: 0.6484 min: 23.9826 max: 26.3593

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.186; Bunge=0, 0, 0; Strength=0.60556; Hardening=25.147

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

-1 0 1 2 3

x 105

-10

-8

-6

-4

-2

0

2x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 1 2 30

5

10

15

20

25

30

35

P 2/3

h

Modulus Fit

Data

Elastic

0 0.2 0.4 0.6 0.80

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 38: Al6061 Nanoindentation results

400F_ 100micron tip_ test 010

65 70 75 800

10

20

Modulus [GPa]

0.94 0.96 0.98 10

10

20

R2

10 20 30 40 500

20

40

Modulus Length [#points]-2 -1.5 -1 -0.5

0

10

20

Hr [nm]

0 0.02 0.04 0.060

20

40

Fit1 Avg.Abs.Res.0 0.05 0.1 0.15 0.2

0

10

20

Fit1 Max.Abs.Res.0 0.1 0.2 0.3 0.4

0

10

20

Fit2 Avg.Abs.Res.0.2 0.4 0.6 0.8 10

10

20

Fit2 Max.Abs.Res.

0.5 0.6 0.7 0.8 0.90

10

20

h change [nm/nm]0.4 0.6 0.8 10

20

40

P change [mN/mN]0.006 0.008 0.01 0.012 0.0140

10

20

Fit4 Avg.Abs.Res.0.015 0.02 0.025 0.030

10

20

Fit4 Max.Abs.Res.

0 0.5 1 1.50

10

20

P* [mN]

5 10 15 20 250

10

20

h* [nm]

0 0.005 0.01 0.015 0.020

10

20

dP [mN]-1 -0.5 0 0.5

0

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 39: Al6061 Nanoindentation results

400F_ 100micron tip_ test 010Estat = mean: 72.9543 median: 72.9222 stdev: 1.6266 min: 70.0865 max: 75.9163

Ystat = mean: 0.4556 median: 0.4465 stdev: 0.0448 min: 0.3839 max: 0.5389

Hstat = mean: 28.2196 median: 28.1243 stdev: 0.8397 min: 26.5468 max: 29.9858

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.5

1

1.5

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.3707; Bunge=0, 0, 0; Strength=0.53241; Hardening=27.4405

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

50

100

150

200

250

300

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0.5 1 1.5 2 2.5

x 105

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 2 2.5-5

0

5

10

15

20

25

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 40: Al6061 Nanoindentation results

525F_ 100micron tip_ test 001

65 70 75 800

10

20

Modulus [GPa]

0.94 0.96 0.98 10

20

40

R2

80 90 100 110 1200

20

40

Modulus Length [#points]-1 -0.8 -0.6 -0.4 -0.2

0

10

20

Hr [nm]

0.005 0.01 0.015 0.020

10

20

Fit1 Avg.Abs.Res.0.02 0.03 0.04 0.05 0.060

10

20

Fit1 Max.Abs.Res.0.1 0.15 0.2 0.250

20

40

Fit2 Avg.Abs.Res.0.4 0.5 0.6 0.7

0

10

20

Fit2 Max.Abs.Res.

0.2 0.3 0.4 0.50

10

20

h change [nm/nm]0.2 0.25 0.3 0.35

0

20

40

P change [mN/mN]7 8 9 10

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.02 0.025 0.03 0.035 0.040

20

40

Fit4 Max.Abs.Res.

0.05 0.1 0.15 0.2 0.250

20

40

P* [mN]

3 4 5 6 70

20

40

h* [nm]

0 0.5 1 1.5 2

x 10-3

0

10

20

dP [mN]-0.6 -0.4 -0.2 0 0.20

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 41: Al6061 Nanoindentation results

Estat = mean: 72.8279 median: 73.1006 stdev: 1.7629 min: 70.0003 max: 75.9999

Ystat = mean: 0.3439 median: 0.3420 stdev: 0.0158 min: 0.3150 max: 0.3783

Hstat = mean: 17.3318 median: 17.3867 stdev: 0.4754 min: 16.5865 max: 18.4025

525F_ 100micron tip_ test 001

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

0.7

0.8

0.9

1

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.2875; Bunge=0, 0, 0; Strength=0.34963; Hardening=17.2816

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

50

100

150

200

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-2

-1.5

-1

-0.5

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.2 0.4 0.6 0.8 1-2

0

2

4

6

8

10

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 42: Al6061 Nanoindentation results

525F_ 100micron tip_ test 002

66 68 70 72 74 760

20

40

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

100

200

R2

50 100 1500

50

100

Modulus Length [#points]-1.2 -1 -0.8 -0.6 -0.4 -0.20

50

100

Hr [nm]

0.005 0.01 0.015 0.020

50

100

Fit1 Avg.Abs.Res.0 0.02 0.04 0.06 0.08 0.1

0

100

200

Fit1 Max.Abs.Res.0.1 0.15 0.2 0.25 0.3 0.350

50

100

Fit2 Avg.Abs.Res.0.2 0.4 0.6 0.8 1 1.20

100

200

Fit2 Max.Abs.Res.

-0.2 0 0.2 0.4 0.60

100

200

h change [nm/nm]0 0.1 0.2 0.3 0.4

0

100

200

P change [mN/mN]5 6 7 8 9 10

x 10-3

0

50

100

Fit4 Avg.Abs.Res.0.01 0.02 0.03 0.04 0.05 0.060

50

100

Fit4 Max.Abs.Res.

0.1 0.2 0.3 0.4 0.50

50

100

P* [mN]

6 7 8 9 10 110

50

100

h* [nm]

0 0.5 1 1.5 2 2.5

x 10-3

0

50

dP [mN]-0.4 -0.2 0 0.2 0.4 0.60

50

100

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 43: Al6061 Nanoindentation results

525F_ 100micron tip_ test 002Estat = mean: 73.0168 median: 72.9951 stdev: 1.7580 min: 70.0013 max: 75.9956

Ystat = mean: 0.3923 median: 0.3923 stdev: 0.0185 min: 0.3468 max: 0.4306

Hstat = mean: 18.0153 median: 17.8977 stdev: 0.6708 min: 17.0777 max: 19.5268

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4679; Bunge=0, 0, 0; Strength=0.36933; Hardening=18.023

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 500 10000

50

100

150

200

250

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-3.5

-3

-2.5

-2

-1.5

-1

-0.5

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.50

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 44: Al6061 Nanoindentation results

525F_ 100micron tip_ test 003

65 70 75 800

10

20

Modulus [GPa]

0.94 0.96 0.98 10

50

R2

50 100 1500

10

20

Modulus Length [#points]-0.9 -0.8 -0.7 -0.6 -0.50

10

20

Hr [nm]

0.005 0.01 0.0150

20

40

Fit1 Avg.Abs.Res.0.025 0.03 0.035 0.04 0.0450

20

40

Fit1 Max.Abs.Res.0.1 0.11 0.12 0.130

20

40

Fit2 Avg.Abs.Res.0.4 0.5 0.6 0.7

0

20

40

Fit2 Max.Abs.Res.

0.1 0.2 0.3 0.4 0.50

20

40

h change [nm/nm]0.1 0.2 0.3 0.4 0.50

10

20

P change [mN/mN]6 7 8 9 10

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.025 0.03 0.035 0.040

50

100

Fit4 Max.Abs.Res.

0.12 0.14 0.16 0.180

10

20

P* [mN]

4.5 5 5.5 60

10

20

h* [nm]

0 0.5 1 1.5 2

x 10-3

0

10

20

dP [mN]-1 -0.5 0 0.5

0

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 45: Al6061 Nanoindentation results

525F_ 100micron tip_ test 003Estat = mean: 72.8329 median: 72.6625 stdev: 1.6899 min: 70.0091 max: 75.9662

Ystat = mean: 0.4241 median: 0.4226 stdev: 0.0182 min: 0.3933 max: 0.4577

Hstat = mean: 17.1184 median: 17.0781 stdev: 0.4141 min: 16.4184 max: 17.9105

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.3119; Bunge=0, 0, 0; Strength=0.42218; Hardening=17.1288

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-500 0 500 10000

50

100

150

200

250

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 5 10 15

x 104

-10

-8

-6

-4

-2

0

2x 10

5

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.2 0.4 0.6 0.8-1

0

1

2

3

4

5

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 46: Al6061 Nanoindentation results

525F_ 100micron tip_ test 004

65 70 75 8010

20

30

Modulus [GPa]

0.94 0.96 0.98 10

100

200

R2

0 50 100 1500

50

Modulus Length [#points]-1.5 -1 -0.5 00

50

100

Hr [nm]

0 0.01 0.02 0.030

50

100

Fit1 Avg.Abs.Res.0 0.02 0.04 0.06 0.08

0

50

100

Fit1 Max.Abs.Res.0.05 0.1 0.15 0.2 0.250

50

100

Fit2 Avg.Abs.Res.0.2 0.4 0.6 0.8 10

50

Fit2 Max.Abs.Res.

0.2 0.4 0.6 0.80

50

h change [nm/nm]0.1 0.2 0.3 0.4 0.50

50

P change [mN/mN]4 6 8 10

x 10-3

0

50

100

Fit4 Avg.Abs.Res.0.01 0.02 0.03 0.040

50

100

Fit4 Max.Abs.Res.

0 0.1 0.2 0.3 0.40

50

100

P* [mN]

6 8 10 120

50

100

h* [nm]

0 1 2 3 4

x 10-3

0

20

40

dP [mN]-1 -0.5 0 0.5

0

50

100

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 47: Al6061 Nanoindentation results

525F_ 100micron tip_ test 004Estat = mean: 72.9655 median: 72.8722 stdev: 1.7495 min: 70.0414 max: 75.9761

Ystat = mean: 0.3900 median: 0.3888 stdev: 0.0169 min: 0.3590 max: 0.4202

Hstat = mean: 17.9959 median: 17.9677 stdev: 0.4532 min: 17.2153 max: 18.7965

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.2

0.4

0.6

0.8

1

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4561; Bunge=0, 0, 0; Strength=0.38674; Hardening=18.0079

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

50

100

150

200

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-4

-3

-2

-1

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 2-5

0

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 48: Al6061 Nanoindentation results

525F_ 100micron tip_ test 005

66 68 70 72 74 760

10

20

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

20

40

R2

70 80 90 100 110 1200

20

40

Modulus Length [#points]-1.5 -1 -0.5 00

20

40

Hr [nm]

0.005 0.01 0.015 0.020

20

40

Fit1 Avg.Abs.Res.0.02 0.04 0.06 0.08 0.10

20

40

Fit1 Max.Abs.Res.0.1 0.15 0.2 0.25 0.3 0.350

50

Fit2 Avg.Abs.Res.0.2 0.4 0.6 0.8 1 1.20

20

40

Fit2 Max.Abs.Res.

0.2 0.3 0.4 0.50

10

20

h change [nm/nm]0.2 0.25 0.3 0.35

0

20

40

P change [mN/mN]7 8 9 10

x 10-3

0

20

40

Fit4 Avg.Abs.Res.0.02 0.025 0.03 0.035 0.040

50

Fit4 Max.Abs.Res.

0 0.1 0.2 0.3 0.4 0.50

50

P* [mN]

2 4 6 8 100

20

40

h* [nm]

0 1 2 3 4 5

x 10-3

0

20

40

dP [mN]-0.6 -0.4 -0.2 0 0.2 0.40

20

40

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 49: Al6061 Nanoindentation results

525F_ 100micron tip_ test 005Estat = mean: 72.9610 median: 73.1697 stdev: 1.8039 min: 70.0003 max: 75.9999

Ystat = mean: 0.3449 median: 0.3440 stdev: 0.0155 min: 0.3150 max: 0.3783

Hstat = mean: 17.3682 median: 17.4043 stdev: 0.4815 min: 16.5865 max: 18.4025

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

0.7

0.8

0.9

1

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4314; Bunge=0, 0, 0; Strength=0.3375; Hardening=17.4237

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

50

100

150

200

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2

x 105

-3

-2.5

-2

-1.5

-1

-0.5

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5-5

0

5

10

15

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 50: Al6061 Nanoindentation results

650F_ 100micron tip_ test 002

65 70 75 800

10

20

Modulus [GPa]

0.98 0.99 1 1.010

50

R2

20 40 60 800

10

20

Modulus Length [#points]-2 -1 0 1

0

10

20

Hr [nm]

0.08 0.1 0.12 0.14 0.160

20

40

Fit1 Avg.Abs.Res.0.2 0.3 0.4 0.50

20

40

Fit1 Max.Abs.Res.0 0.1 0.2 0.3 0.4

0

10

20

Fit2 Avg.Abs.Res.0 0.5 1 1.5

0

10

20

Fit2 Max.Abs.Res.

0.7 0.8 0.9 10

10

20

h change [nm/nm]0.4 0.5 0.6 0.7 0.80

20

40

P change [mN/mN]0.02 0.03 0.04 0.050

10

20

Fit4 Avg.Abs.Res.0.04 0.05 0.06 0.07 0.080

10

20

Fit4 Max.Abs.Res.

0.8 1 1.2 1.40

10

20

P* [mN]

30 35 40 450

10

20

h* [nm]

0 0.005 0.01 0.0150

10

20

dP [mN]-0.5 0 0.5 1 1.50

10

20

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 51: Al6061 Nanoindentation results

650F_ 100micron tip_ test 002Estat = mean: 73.0756 median: 72.9917 stdev: 1.6628 min: 70.1255 max: 75.9698

Ystat = mean: 0.2518 median: 0.2515 stdev: 0.0119 min: 0.2208 max: 0.2790

Hstat = mean: 12.9052 median: 12.8873 stdev: 0.7722 min: 11.7981 max: 14.2977

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

0.7

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.4988; Bunge=0, 0, 0; Strength=0.25718; Hardening=12.4377

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

20

40

60

80

100

120

140

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3

x 105

-12

-10

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 2-5

0

5

10

15

20

25

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.030

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 52: Al6061 Nanoindentation results

650F_ 100micron tip_ test 003

Page 53: Al6061 Nanoindentation results

650F_ 100micron tip_ test 003Estat = mean: 72.8141 median: 72.5877 stdev: 1.7410 min: 70.0232 max: 75.9629

Ystat = mean: 0.2503 median: 0.2504 stdev: 0.0100 min: 0.2326 max: 0.2741

Hstat = mean: 13.3240 median: 13.2591 stdev: 0.4620 min: 12.0619 max: 14.2475

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

0.7

0.8

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.2711; Bunge=0, 0, 0; Strength=0.25215; Hardening=13.2591

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 500 10000

50

100

150

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3

x 105

-14

-12

-10

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 2-5

0

5

10

15

20

25

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.03 0.040

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 54: Al6061 Nanoindentation results

650F_ 100micron tip_ test 004

65 70 75 800

5

10

Modulus [GPa]

0.98 0.99 1 1.010

20

40

R2

20 40 60 800

10

20

Modulus Length [#points]-2 -1 0 1

0

10

20

Hr [nm]

0.1 0.12 0.14 0.160

20

40

Fit1 Avg.Abs.Res.0.25 0.3 0.35 0.4 0.450

10

20

Fit1 Max.Abs.Res.0 0.1 0.2 0.3 0.4

0

10

20

Fit2 Avg.Abs.Res.0 0.5 1 1.5

0

10

20

Fit2 Max.Abs.Res.

0.75 0.8 0.85 0.9 0.950

5

10

h change [nm/nm]0.4 0.5 0.6 0.7 0.80

10

20

P change [mN/mN]0.02 0.03 0.04 0.050

5

10

Fit4 Avg.Abs.Res.0.045 0.05 0.055 0.060

5

10

Fit4 Max.Abs.Res.

0.7 0.8 0.9 10

5

10

P* [mN]

54 56 58 600

5

10

h* [nm]

0 0.005 0.010

10

20

dP [mN]-0.5 0 0.5 10

10

20

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 55: Al6061 Nanoindentation results

650F_ 100micron tip_ test 004Estat = mean: 72.7263 median: 72.4234 stdev: 1.7910 min: 70.0506 max: 75.9400

Ystat = mean: 0.2271 median: 0.2261 stdev: 0.0108 min: 0.1959 max: 0.2459

Hstat = mean: 12.3714 median: 12.0507 stdev: 0.6598 min: 11.5263 max: 13.4687

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

0.7

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.1896; Bunge=0, 0, 0; Strength=0.23049; Hardening=12.0506

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

20

40

60

80

100

120

140

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3

x 105

-14

-12

-10

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 2-5

0

5

10

15

20

25

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.030

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 56: Al6061 Nanoindentation results

650F_ 100micron tip_ test 005

65 70 75 800

5

10

Modulus [GPa]

0.96 0.98 1 1.020

20

40

R2

20 40 60 800

5

10

Modulus Length [#points]-1 -0.5 0 0.5

0

5

10

Hr [nm]

0.08 0.1 0.12 0.14 0.160

10

20

Fit1 Avg.Abs.Res.0.2 0.25 0.3 0.35 0.40

10

20

Fit1 Max.Abs.Res.0.05 0.1 0.15 0.2 0.250

5

10

Fit2 Avg.Abs.Res.0 0.5 1

0

10

20

Fit2 Max.Abs.Res.

0.75 0.8 0.85 0.9 0.950

5

10

h change [nm/nm]0.4 0.5 0.6 0.7 0.80

5

10

P change [mN/mN]0.025 0.03 0.035 0.04 0.0450

5

10

Fit4 Avg.Abs.Res.0.05 0.055 0.06 0.0650

5

10

Fit4 Max.Abs.Res.

0.55 0.6 0.65 0.7 0.750

5

10

P* [mN]

31 32 33 34 350

5

10

h* [nm]

0 2 4 6 8

x 10-3

0

5

10

dP [mN]-0.5 0 0.5 10

5

10

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 57: Al6061 Nanoindentation results

650F_ 100micron tip_ test 005

Estat = mean: 73.0497 median: 72.7548 stdev: 1.8111 min: 70.0597 max: 75.9970

Ystat = mean: 0.2244 median: 0.2263 stdev: 0.0123 min: 0.1897 max: 0.2476

Hstat = mean: 13.1493 median: 13.0770 stdev: 0.4404 min: 12.2847 max: 13.9221

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.467; Bunge=0, 0, 0; Strength=0.23406; Hardening=12.931

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 6000

20

40

60

80

100

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2 2.5

x 105

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5-5

0

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.030

1000

2000

3000

4000

5000

6000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 58: Al6061 Nanoindentation results

650F_ 100micron tip_ test 006

66 68 70 72 74 760

10

20

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

20

40

R2

20 25 30 35 40 450

10

20

Modulus Length [#points]-1 -0.5 0 0.5 1

0

10

20

Hr [nm]

0.1 0.2 0.3 0.4 0.50

10

20

Fit1 Avg.Abs.Res.0 0.5 1 1.5 2

0

10

20

Fit1 Max.Abs.Res.0.1 0.2 0.3 0.4 0.5 0.60

10

20

Fit2 Avg.Abs.Res.0 0.5 1 1.5 2

0

10

20

Fit2 Max.Abs.Res.

0.75 0.8 0.85 0.9 0.950

20

40

h change [nm/nm]0.65 0.7 0.75 0.8

0

10

20

P change [mN/mN]0.045 0.05 0.055 0.06 0.065 0.070

10

20

Fit4 Avg.Abs.Res.0.06 0.07 0.08 0.09 0.1 0.110

10

20

Fit4 Max.Abs.Res.

0 1 2 3 4 50

10

20

P* [mN]

60 70 80 90 100 1100

10

20

h* [nm]

0 0.01 0.02 0.030

10

20

dP [mN]0 0.5 1 1.5 2 2.5

0

10

20

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 59: Al6061 Nanoindentation results

650F_ 100micron tip_ test 006

Estat = mean: 72.5025 median: 72.0208 stdev: 1.7646 min: 70.0303 max: 75.9951

Ystat = mean: 0.1528 median: 0.1565 stdev: 0.0120 min: 0.1219 max: 0.1704

Hstat = mean: 14.1212 median: 13.9646 stdev: 0.8057 min: 12.9491 max: 15.8711

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

0.7

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=68.9422; Bunge=0, 0, 0; Strength=0.16582; Hardening=13.5432

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

-200 0 200 400 600 8000

20

40

60

80

100

120

140

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 1 2 3 4

x 105

-2.5

-2

-1.5

-1

-0.5

0

0.5x 10

7

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5 20

5

10

15

20

25

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.030

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 60: Al6061 Nanoindentation results

775F_ 100micron tip_ test 002

66 68 70 72 74 760

5

10

Modulus [GPa]

0.95 0.96 0.97 0.98 0.99 10

10

20

R2

30 35 40 45 50 550

5

10

Modulus Length [#points]-1 -0.5 0 0.5 1

0

5

10

Hr [nm]

0.08 0.1 0.12 0.14 0.160

10

20

Fit1 Avg.Abs.Res.0.3 0.32 0.34 0.36 0.38

0

10

20

Fit1 Max.Abs.Res.0.1 0.15 0.2 0.250

5

10

Fit2 Avg.Abs.Res.0.2 0.4 0.6 0.8 10

10

20

Fit2 Max.Abs.Res.

0.86 0.88 0.9 0.92 0.940

5

10

h change [nm/nm]0.55 0.6 0.65 0.7 0.750

5

10

P change [mN/mN]0.02 0.03 0.04 0.05 0.06 0.070

5

10

Fit4 Avg.Abs.Res.0.04 0.06 0.08 0.10

10

20

Fit4 Max.Abs.Res.

0.5 0.6 0.7 0.8 0.9 10

5

10

P* [mN]

56 58 60 62 64 660

5

10

h* [nm]

0 0.002 0.004 0.006 0.008 0.010

5

10

dP [mN]-0.5 0 0.5 1 1.5 20

5

10

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 61: Al6061 Nanoindentation results

775F_ 100micron tip_ test 002

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.0392; Bunge=0, 0, 0; Strength=0.15987; Hardening=11.39

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

20

40

60

80

100

120

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2 2.5

x 105

-14

-12

-10

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.5-5

0

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.030

2000

4000

6000

8000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Estat = mean: 72.6774 median: 72.4660 stdev: 1.5328 min: 70.1452 max: 75.7897

Ystat = mean: 0.1801 median: 0.1808 stdev: 0.0080 min: 0.1588 max: 0.2022

Hstat = mean: 10.8999 median: 10.8444 stdev: 0.3716 min: 10.1605 max: 11.7637

Page 62: Al6061 Nanoindentation results

775F_ 100micron tip_ test 004

66 68 70 72 74 760

5

10

Modulus [GPa]

0.96 0.97 0.98 0.99 1 1.010

10

20

R2

20 30 40 50 60 700

5

10

Modulus Length [#points]-1.5 -1 -0.5 0 0.5 10

5

10

Hr [nm]

0.1 0.12 0.14 0.160

5

10

Fit1 Avg.Abs.Res.0.25 0.3 0.35 0.4 0.450

5

10

Fit1 Max.Abs.Res.0.1 0.15 0.2 0.250

5

10

Fit2 Avg.Abs.Res.0.4 0.5 0.6 0.7

0

5

10

Fit2 Max.Abs.Res.

0.8 0.85 0.9 0.95 10

2

4

h change [nm/nm]0.5 0.6 0.7 0.8 0.90

5

10

P change [mN/mN]0.02 0.03 0.04 0.05 0.06 0.070

10

20

Fit4 Avg.Abs.Res.0.04 0.05 0.06 0.07 0.08 0.090

10

20

Fit4 Max.Abs.Res.

0.7 0.8 0.9 1 1.10

10

20

P* [mN]

44 46 48 50 52 540

5

10

h* [nm]

0 0.002 0.004 0.006 0.008 0.010

5

10

dP [mN]-1 -0.5 0 0.5 1 1.5

0

5

10

dH [nm]

effective

sample

Fit1

Fit2

Fit3

Page 63: Al6061 Nanoindentation results

775F_ 100micron tip_ test 004Estat = mean: 72.9440 median: 72.5348 stdev: 1.7310 min: 70.2726 max: 75.8985

Ystat = mean: 0.1815 median: 0.1793 stdev: 0.0162 min: 0.1483 max: 0.2122

Hstat = mean: 11.4562 median: 11.0910 stdev: 0.7168 min: 10.4900 max: 12.6142

0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.040

0.1

0.2

0.3

0.4

0.5

0.6

Ind. Strain

Ind.

Str

ess

[GP

a]

Es=69.1715; Bunge=0, 0, 0; Strength=0.18232; Hardening=10.8001

Stress-StrainModulus Line

Hardening Fit

Strain Offset

Modulus Fit Data

Hardening Fit DataYield Point

0 200 400 600 8000

20

40

60

80

100

120

displacement / nm

load

/ m

N

Load Vs. Displacement

Raw Data

0 Pt. Data

0 0.5 1 1.5 2 2.5

x 105

-12

-10

-8

-6

-4

-2

0x 10

6

S

P2/

3-S

h

Zero Point Fit

Raw Data

0 Pt. Data

0 0.5 1 1.50

5

10

15

20

P 2/3

h

Modulus Fit

Data

Elastic

0 0.01 0.02 0.030

1000

2000

3000

4000

5000

6000

7000

Strain

Con

tact

Rad

ius

/ nm

Strain Vs. Contact Radius

Data

Elastic

Page 64: Al6061 Nanoindentation results

775F_ 100micron tip_ test 005

Page 65: Al6061 Nanoindentation results

775F_ 100micron tip_ test 005Estat = mean: 73.0240 median: 73.0903 stdev: 1.7293 min: 70.0061 max: 75.9250

Ystat = mean: 0.2102 median: 0.2100 stdev: 0.0102 min: 0.1834 max: 0.2314

Hstat = mean: 9.9928 median: 9.9663 stdev: 0.2857 min: 9.4651 max: 10.6556

Page 66: Al6061 Nanoindentation results

775F_ 100micron tip_ test 007

Page 67: Al6061 Nanoindentation results

775F_ 100micron tip_ test 007

Page 68: Al6061 Nanoindentation results

775F_ 100micron tip_ test 010

Page 69: Al6061 Nanoindentation results

775F_ 100micron tip_ test 010

Page 70: Al6061 Nanoindentation results

Elastic module Yield strength (GPa) HardeningAs received

400 F 55.73153 0.422567 20.59428525 F 56.33968 0.2724 14.30632650 F775 F