![Page 1: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/1.jpg)
Claude Ployaert
Concrete Technology Engineer
Inter-Beton
Steven Schaerlaekens
Technical Support Manager
Holcim België
Leden van de Commissie E104
Voor FedBeton
![Page 2: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/2.jpg)
De nieuwe normen
NBN EN 206 en NBN B 15-001
Via NBN: enkel EN, FR, DEZie gebundelde versie voor NL !
![Page 3: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/3.jpg)
+ =
![Page 4: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/4.jpg)
Agenda
1 – Omgevingsklassen en milieuklassen
2 – Specificatie van de druksterkteklasse
3 – Eisen met betrekking tot de bestanddelen
4 – Specificatie van beton
5 – Levering van beton
6 – Conformiteitscontrole van beton
7 – Beton voor speciale geotechnische werken
8 – Maatregelen ter preventie van alkali-silica reactie (ASR)
9 – Wateropslorping door onderdompeling
10 – Nieuwe versie TRA 550
![Page 5: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/5.jpg)
1 – OMGEVINGSKLASSEN en MILIEUKLASSEN
![Page 6: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/6.jpg)
Omgevingsklassen en milieuklassen
XF3 in plaats van XF1
horizontale verticaleoppervlakken
4.1 en Bijlage F
![Page 7: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/7.jpg)
E I
EE3
ES2
EE2
ES4
ES3
E 0
Zeewater
Eau de mer
EE4
Zwembad (Cl-)
Piscine (Cl-)
ES3
EE1
Binnenland
Arrière-pays
Zeewateromgeving
Environnement marin
ES1
Brak water
Eau saumâtre
EE4
Zeelucht + vorst
Air marine + gel
Geen vorst
Pas de gel
Vorst + regen
Gel + pluie
EE1
EE4
Omgevingsklassen en milieuklassen
![Page 8: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/8.jpg)
Omgevingsklassen en milieuklassen
+ =
![Page 9: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/9.jpg)
Omgevingsklassen en milieuklassen
SR-cement
Eventueel
aangeven dat het
betontype met
ingebrachte lucht
nodig is
![Page 10: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/10.jpg)
2 – SPECIFICATIE VAN DE DRUKSTERKTEKLASSE
![Page 11: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/11.jpg)
C fckcyl/fckcub na 28 dagen
In specifieke situaties kan de karakteristieke druksterkte op een andere
ouderdom dan 28 dagen gedeclareerd worden (kan interessant zijn voor
massieve constructies)
Specificatie van de druksterkteklasse
4.3.1 en 5.5.1.2
Aanduiding: CX/Y (zd) �C35/45 (90d)�C30/37 (56d)�…
![Page 12: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/12.jpg)
Specificatie van de druksterkteklasse
5.5.1.2
�Proctor�Vibrating hammer�Vibrocompression�Axial compression
![Page 13: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/13.jpg)
3 – EISEN MET BETREKKING TOT DE BESTANDDELEN
![Page 14: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/14.jpg)
Algemene gebruiksgeschiktheid
![Page 15: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/15.jpg)
Specifieke gebruiksgeschiktheid
![Page 16: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/16.jpg)
NBN B15-100(2018)
![Page 17: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/17.jpg)
Cement : specifieke gebruiksgeschiktheid
5.1.2
![Page 18: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/18.jpg)
Cement : specifieke gebruiksgeschiktheid
5.1.2
![Page 19: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/19.jpg)
Tabel 5-ANB — Gebruiksgeschiktheid voor gewapend en voorgespannen beton voor niveau I en niveau II van de cementen volgens NBN EN 197-1 en de cement-t oevoegsel type II combinaties in functie van de omgevingsklassen
![Page 20: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/20.jpg)
Gerecycleerde granulaten
Twee types gerecycleerde granulaten worden gedefinieerd:
![Page 21: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/21.jpg)
Twee types gerecycleerde granulaten worden gedefinieerd:
Gerecycleerde granulaten
![Page 22: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/22.jpg)
Het gebruik van granulaten
De vorstbestandheid kan eveneens worden aangetoond via NBN B 15-100
![Page 23: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/23.jpg)
Het gebruik van gerecycleerde granulaten
![Page 24: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/24.jpg)
� Vervanging van tabel E.2 uit bijlage E van de NBN EN 206
� Betongranulaat type A+ en menggranulaat type B+ mogen niet gecombineerd worden
� Voor een hoger vervangingspercentage of gebruik in andere omgevings- en druksterkteklassen alsook in voorgespannen beton dient de algemene en specifieke gebruiksgeschiktheid aangetoond te worden voor de beoogde betonsamenstelling en het beoogde gebruik
� Betongranulaat type A+ mag gebruikt worden t/m druksterkteklasse C30/37� Menggranulaat type B+ mag gebruikt worden t/m druksterkteklasse C20/25
Het gebruik van gerecycleerde granulaten
![Page 25: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/25.jpg)
Het gebruik van gerecycleerde granulaten
![Page 26: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/26.jpg)
Toevoegsels - Algemeen
![Page 27: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/27.jpg)
Nieuw
Het gebruik van vliegas
![Page 28: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/28.jpg)
Het gebruik van vliegas
![Page 29: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/29.jpg)
Het gebruik van LMA
![Page 30: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/30.jpg)
Het gecombineerd gebruik van vliegas en LMA
![Page 31: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/31.jpg)
�Hulpstof initieel voorzien in het recept : watergehalte moet meegerekendworden bij de berekening van de (theoretische) W/C
�Hulpstof niet voorzien in het recept : watergehalte van deze hulpstof moetniet meegerekend worden tenzij de hoeveelheid > 3,0 l/m³
Het gebruik van hulpstoffen
![Page 32: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/32.jpg)
Het gebruik van vezels
![Page 33: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/33.jpg)
Het gebruik van vezels
![Page 34: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/34.jpg)
Het gebruik van vezels
![Page 35: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/35.jpg)
Het gebruik van vezels
![Page 36: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/36.jpg)
� TRA 550 v4.0
Het gebruik van vezels
![Page 37: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/37.jpg)
4 – SPECIFICATIE VAN BETON
![Page 38: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/38.jpg)
Specificatie van beton
Cement SR of HSR !
6.2.2
![Page 39: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/39.jpg)
6.2.2
Specificatie van beton
![Page 40: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/40.jpg)
Specificatie van beton
![Page 41: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/41.jpg)
Specificatie van beton - ZVB
� TRA 550 v4.0
(Zelfcontrole: geen enkele tolerantie toegestaan op deze klassen)
![Page 42: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/42.jpg)
5 – LEVERING VAN BETON
![Page 43: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/43.jpg)
De leveringsbon
7.3
![Page 44: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/44.jpg)
6 – CONFORMITEITSCONTROLE VAN BETON
![Page 45: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/45.jpg)
Conformiteitscontrole van vers beton
-20 / + 20 mm bij het begin van het
lossen = 1e m³
8.2
� Gedaan met AQL
voor consistentie
� Individuele
evaluatie
![Page 46: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/46.jpg)
Conformiteitscontrole van verhard beton
![Page 47: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/47.jpg)
7 – BETON VOOR SPECIALE GEOTECHNISCHE WERKEN
![Page 48: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/48.jpg)
Algemeen
![Page 49: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/49.jpg)
Specifiek voor palen
![Page 50: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/50.jpg)
Specifiek voor diepwanden
![Page 51: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/51.jpg)
Algemeen consistentie
WG FABA / ABEF / FedBeton / WTCB: S5 (≥ 220 mm
![Page 52: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/52.jpg)
Algemeen filtratieverlies
#% (m/m water) #ml (op +/- 2 liter beton 8 mm)
![Page 53: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/53.jpg)
8 – MAATREGELEN TER PREVENTIE VAN
ALKALI-SILICA REACTIE (ASR)
![Page 54: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/54.jpg)
Preventie ASR
� Verantwoordelijkheid van de voorschrijver : het risico evalueren in functie van
de economische en maatschappellijke kosten � het ASR-PREVENTIENIVEAU
(PREV) vastleggen.
NIVEAU Omschrijving Voorbeelden
PREV1 Gevolgen van ASR zeer beperkt en
aanvaardbaar
Vervangbare elementen, tijdelijke
constructies …
PREV2 Gevolgen van ASR weinig aanvaardbaar Constructief beton
PREV3 Gevolgen van ASR niet aanvaardbaar Grote en/of belangrijke bouwwerken
(bruggen, kaaimuren …)
![Page 55: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/55.jpg)
�De blootstelling van het bouwelement is bepalend voor het optreden en de
graad van voortschrijding van de reactie. Deze factor is verbonden met de ASR-
BLOOTSTELLINGSCATEGORIE (AR), in nauw verband met de omgevings- of
milieuklassen.
E0 AR1
EA
EA1 AR2
EA2 AR2
EA3 AR2
EI AR1
EE
EE1 AR2
EE2 AR2
EE3 AR2
EE4 AR3
ES
ES1 AR2
ES2 AR2
ES3 AR2
ES4 AR3
AR
AR1 Bouwdelen in droge binnenomgeving,
zonder blootstelling aan externe bronnen
van vocht
AR2 Bouwdelen in vochtige binnenomgevingen
en buitenomgevingen, ondergedompeld in
(zee)water of in contact met niet-agressieve
grond
AR3 Bouwdelen in vochtig milieu blootgesteld
aan alkaliën (bijvoorbeeld dooizouten) of
aan wisselend vocht-droog cycli met
zeewater of brak water
Preventie ASR
= default
![Page 56: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/56.jpg)
�In functie van het gedefinieerde ASR-preventieniveau en de geselecteerde ASR-
blootstellings-categorie dienen de gepaste preventieve maatregelen genomen te
worden. Vier verschillende maatregelen worden beschreven ter preventie van
de schadelijke gevolgen van de alkali -silica reactie.
AR1 AR2 AR3
PREV1 Geen Geen Geen
PREV2 Geen 1 of 2 of 3 of 4 1 of 2 of 3 of 4
PREV3 Geen 1 of 3 of 4 1 of 3* of 4*
1. Gebruik van niet-reactieve granulaten
2. Gebruik van een LA-cement (conform aan de NBN B 12-109)
3. Beperken van het alkaligehalte van het beton (via alkalibalans)
4. Voorafgaandelijk uitvoeren van performantieproeven in labo
Indien de voorschrijver geen preventieniveau opgeeft, dient de beton-
producent standaard uit te gaan van het preventieniveau PREV2 en de AR-
klasse die overeenkomt met de gespecifieerde omgevingsklasse
* Met strengere eisen bij deze maatregelen
Preventie ASR
![Page 57: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/57.jpg)
� 4 mogelijke preventiemaatregelen
1. Gebruik van granulaten met geattesteerde declaratie van niet-reactiviteit
Preventie ASR
![Page 58: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/58.jpg)
� 4 mogelijke preventiemaatregelen
2. Gebruik van een LA-cement volgens NBN B 12-109, zonder opmaak van een
alkalibalans
Preventie ASR
![Page 59: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/59.jpg)
� 4 mogelijke preventiemaatregelen
3. Beperken van het alkali-gehalte van beton tot een vastgelegde waarde
Preventie ASR
![Page 60: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/60.jpg)
� 4 mogelijke preventiemaatregelen
OFWEL
Preventie ASR
![Page 61: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/61.jpg)
� TRA 550 v4.0Preventie ASR
/ zanden / toevoegsels Type I
![Page 62: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/62.jpg)
� 4 mogelijke preventiemaatregelen
Preventie ASR
![Page 63: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/63.jpg)
� 4 mogelijke preventiemaatregelen
Preventie ASR
![Page 64: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/64.jpg)
� 4 mogelijke preventiemaatregelen
Preventie ASR
![Page 65: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/65.jpg)
4. Voorafgaandelijk uitvoeren van zwelproeven
- Gemodificeerde Oberholster proef
- NF P 18-454 (methodologie) en FD P 18-456 (criteria)
� 4 mogelijke preventiemaatregelen
Preventie ASR
![Page 66: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/66.jpg)
Voorbeeld – T(0,50)
![Page 67: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/67.jpg)
Voorbeeld – T(0,45)
![Page 68: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/68.jpg)
Voorbeeld – T(0,45) mix CEM
![Page 69: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/69.jpg)
9 – WATEROPSLORPING DOOR ONDERDOMPELING
%100.m
mmA
droog
droogvochtig in−
=
![Page 70: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/70.jpg)
Wateropslorping door onderdompeling
Nieuwe klasse !
![Page 71: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/71.jpg)
Deze waarden gelden voor Dmax ≥ 20 mm !!
Wateropslorping door onderdompeling
![Page 72: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/72.jpg)
10 - NIEUWE VERSIE TRA 550
![Page 73: Claude Ployaert ConcreteTechnologyEngineer Inter-Beton...Algemeen filtratieverlies #% (m/m water) #ml (op +/- 2 liter beton 8 mm) 8 –MAATREGELEN TER PREVENTIE VAN ALKALI-SILICA REACTIE](https://reader033.vdocuments.net/reader033/viewer/2022051810/601a8065e7839e735b387e2a/html5/thumbnails/73.jpg)