    WELDING DEFECTS

    1.ROOT OFFSET

    2.EXCESS PENETRATION

    TITLE : WELDING INSPECTOR WI : 21

  • 8/3/2019 Weld Defects Flim

    6/21

    WELDING DEFECTS

    3. LACK OF PENETRATION

    4. LACK OF SIDE WALL FUSION

    TITLE : WELDING INSPECTOR WI : 22

  • 8/3/2019 Weld Defects Flim

    7/21

    WELDING DEFECTS

    5. WELD OVERLAP

    6. EXCESSIVE RE-INFORCEMENT

    TITLE : WELDING INSPECTOR WI : 23

  • 8/3/2019 Weld Defects Flim

    8/21

    WELDING DEFECTS

    7. UNDERFILL

    8. UNDERCUT

    TITLE : WELDING INSPECTOR WI : 24

  • 8/3/2019 Weld Defects Flim

    9/21

    WELDING DEFECTS

    9. CRACKS

    TITLE : WELDING INSPECTOR WI : 25

  • 8/3/2019 Weld Defects Flim

    10/21

    WELDING DEFECTS

    10. DISTRIBUTED & CLUSTER POROSITY

    TITLE : WELDING INSPECTOR WI : 26

  • 8/3/2019 Weld Defects Flim

    11/21

    WELDING DEFECTS

    10. INCLUSIONS

    11.INTER-BEAD CREVICE/VALLEY

    TITLE : WELDING INSPECTOR WI : 27

  • 8/3/2019 Weld Defects Flim

    12/21

    WELDING DEFECTS

    12.SUCKBACK

    14. ROOT OXIDATION

    TITLE : WELDING INSPECTOR WI : 28

  • 8/3/2019 Weld Defects Flim

    13/21

    WELDING DEFECTS

    15.LAMELLAR TEARS

    TITLE : WELDING INSPECTOR WI : 29

  • 8/3/2019 Weld Defects Flim

    14/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    POROSITY

    TITLE : WELDING INSPECTOR WI : 63

  • 8/3/2019 Weld Defects Flim

    15/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    CLUSTER POROSITY

    TITLE : WELDING INSPECTOR WI : 64

  • 8/3/2019 Weld Defects Flim

    16/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    SLAG INCLUSIONS

    TITLE : WELDING INSPECTOR WI : 65

  • 8/3/2019 Weld Defects Flim

    17/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    INCOMPLETE PENETRATION (IP) OR LACK OFPENETRATION (LOP)

    TITLE : WELDING INSPECTOR WI : 66

  • 8/3/2019 Weld Defects Flim

    18/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    INCOMPLETE FUSION

    TITLE : WELDING INSPECTOR WI : 67

  • 8/3/2019 Weld Defects Flim

    19/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    INTERNAL OR ROOT UNDERCUT

    TITLE : WELDING INSPECTOR WI : 68

  • 8/3/2019 Weld Defects Flim

    20/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    CRACKING

    TITLE : WELDING INSPECTOR WI : 69

  • 8/3/2019 Weld Defects Flim

    21/21

    RADIOGRAPHIC INDICATIONS FOR WELDING

    TUNGSTEN INCLUSIONS .