fractography resource - [email protected] 1 examples of fractography in other materials...

16
Fractography Resource - mjames@plymouth. ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James [email protected]. uk Department of Mechanical & Marine Engineering University of Plymouth Drake Circus, Plymouth PL4 8AA ENGLAND

Upload: russell-beardsley

Post on 15-Jan-2016

238 views

Category:

Documents


0 download

TRANSCRIPT

Page 1: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Examples of Fractography in Other Materials

Professor M Neil [email protected]

Department of Mechanical & Marine Engineering

University of Plymouth

Drake Circus, Plymouth PL4 8AA

ENGLAND

Page 2: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Contents – Use the hyperlinks to navigate around this resource

WC-Co : Compression and tensile fatigue

316L stainless steel – SCC

Fatigue in polycarbonate

Fast fracture in polycarbonate

Page 3: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

WC-Co : Compression and tensile fatigue

6% Co Grade T6

Rupture = 2190 MPa - average grain size = 1.8 m

The line indicates the transition between regions of compression fatigue (lower half) and tensile fatigue (upper half)

Original magnification shown by micron bar

Page 4: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

WC-Co : Compression and tensile fatigue

6% Co Grade T6

Rupture = 2190 MPa - average grain size = 1.8 m

Compression fatigue at higher magnification – WC grains are rounded and Co tear ridges are less frequent

Original magnification shown by micron bar

Page 5: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

WC-Co : Compression and tensile fatigue

6% Co Grade T6

Rupture = 2190 MPa - average grain size = 1.8 m

Tensile fatigue at higher magnification – WC grains are more angular and Co tear ridges are more evident

Original magnification shown by micron bar

Back to Contents

Page 6: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

316L stainless steel - SCC

0.033C 1.44Mn 0.44Si 18.4Cr 8.6Ni 0.016P 0.010S

YS = 205 MPa in annealed state : Vickers hardness 235

2 mm thick, 120 mm diameter seam welded pipe used to transport glucose solution

Cracking associated with weld – inner surface of pipe shown here – significant crack branching

Page 7: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

316L stainless steel - SCC

0.033C 1.44Mn 0.44Si 18.4Cr 8.6Ni 0.016P 0.010S

YS = 205 MPa in annealed state : Vickers hardness 235

2 mm thick, 120 mm diameter seam welded pipe used to transport glucose solution

Cracking associated with weld – outer surface of pipe shown here – less crack branching

Implication: glucose is cause of problem, not external lagging

Page 8: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

316L stainless steel - SCC

0.033C 1.44Mn 0.44Si 18.4Cr 8.6Ni 0.016P 0.010S

YS = 205 MPa in annealed state : Vickers hardness 235

2 mm thick, 120 mm diameter seam welded pipe used to transport glucose solution

Fracture surface shows brittle appearance – not fatigue crack growth

Page 9: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

316L stainless steel - SCC

0.033C 1.44Mn 0.44Si 18.4Cr 8.6Ni 0.016P 0.010S

YS = 205 MPa in annealed state : Vickers hardness 235

2 mm thick, 120 mm diameter seam welded pipe used to transport glucose solution

Have 'feathery' cleavage facets present

Implication: SCC, although detrimental species not clear

Page 10: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

316L stainless steel - SCC

0.033C 1.44Mn 0.44Si 18.4Cr 8.6Ni 0.016P 0.010S

YS = 205 MPa in annealed state : Vickers hardness 235

2 mm thick, 120 mm diameter seam welded pipe used to transport glucose solution

Pipe operates at 60°C – diagram indicates that chloride SCC occurs at this temperature in acid solutions with 104 ppm of chlorides present

Back to Contents

Page 11: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Fatigue in polycarbonate

YS = 20 MPa (initial cyclic yield) - annealed state – 2 mm thick plate

R = 0.5

Notch root is at the left of the picture

Page 12: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Fatigue in polycarbonate

YS = 20 MPa (initial cyclic yield) - annealed state – 2 mm thick plate

R = 0.5

Near the notch root

Page 13: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Fatigue in polycarbonate

YS = 20 MPa (initial cyclic yield) - annealed state – 2 mm thick plate

R = 0.5

Near the notch root

The marks are not fatigue striations

Page 14: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Fatigue in polycarbonate

YS = 20 MPa (initial cyclic yield) - annealed state – 2 mm thick plate

R = 0.5

This position is 7.5 mm from the notch root

Page 15: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Fatigue in polycarbonate

YS = 20 MPa (initial cyclic yield) - annealed state – 2 mm thick plate

R = 0.5

This position is 17.5 mm from the notch root

The marks are not fatigue striations – they probably relate to craze size ahead of the crack tip

Page 16: Fractography Resource - mjames@plymouth.ac.uk 1 Examples of Fractography in Other Materials Professor M Neil James mjames@plymouth.ac.uk Department of

Fractography Resource - [email protected]

Fast fracture in polycarbonate

YS = 20 MPa (initial cyclic yield) - annealed state – 2 mm thick plate

This shows typical fast fracture in the PC

Features are very similar to fatigue

Back to Contents