fractography: the way things fracture -...
TRANSCRIPT
![Page 1: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/1.jpg)
Fractography: The Way Things Fracture
S.K. BhaumikMaterials Science Division
Council of Scientific & Industrial Research (CSIR)
National Aerospace LaboratoriesBangalore 560 017
![Page 2: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/2.jpg)
June 28, 2012 National Aerospace Laboratories
Outline…
Introduction
Classification of fracture
Fracture features Macroscopic
Microscopic
Identification of fracture modes
Applications Examples from failure analysis
Conclusions
![Page 3: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/3.jpg)
National Aerospace Laboratories
Fractography: definition
Fractography is the study of fracture surfaces of materials
Signatures of fracture process
Characteristic features
Examination of fracture surfaces to determine mode and cause of fracture
Macroscopic features: smoothness and markings observable with naked eyes or optical microscope
Microscopic features: detailed information by using electron microscope
June 28, 2012
![Page 4: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/4.jpg)
National Aerospace Laboratories
Fractography: frequent use
Determine the cause of failure in engineering structures or products
Failure analysis
Forensic engineering
Materials science research
Study of mechanical response of materials
Study of crack growth behaviour
………………………
June 28, 2012
![Page 5: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/5.jpg)
National Aerospace Laboratories
Fractography: objectives
Mode of fracture
Fatigue
Stress corrosion cracking
Hydrogen embrittlement etc
Reason for crack initiation
Stress concentration
Material defects
Corrosion etc
Study of crack growth rate
………………
June 28, 2012
![Page 6: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/6.jpg)
National Aerospace Laboratories
Fracture in metals
Non-fluctuating stresses
Fluctuating stresses
Mechanical
Chemical Thermal
June 28, 2012
![Page 7: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/7.jpg)
National Aerospace Laboratories
Fracture in metals
Non-fluctuating stresses
Mechanical or overload: tension, compression, bending, torsion, shear……
Chemical: stress corrosion, hydrogen embrittlement, liquid metal embrittlement, exfoliation……
Thermal: creep……
June 28, 2012
![Page 8: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/8.jpg)
National Aerospace Laboratories
Fracture in metals
Fluctuating stresses
Mechanical or overload: fatigue (HCF, LCF), fretting, fretting-fatigue, wear……
Chemical: corrosion fatigue…..
Thermal: fatigue……
June 28, 2012
![Page 9: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/9.jpg)
National Aerospace Laboratories
Fracture in metals…engineering importance
Mechanical
Ductile, brittle, fatigue
Environmental
Corrosion, corrosion-erosion
Mechanical-environmental
Stress corrosion cracking, hydrogen embrittlement, corrosion fatigue
June 28, 2012
![Page 10: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/10.jpg)
National Aerospace Laboratories
Fracture in metals…engineering importance
Static overload fracture
Ductile, brittle
Progressive fracture
Fatigue, stress corrosion cracking, hydrogen embrittlement, stress-rupture
June 28, 2012
![Page 11: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/11.jpg)
National Aerospace Laboratories
Fracture in metals…statistics
Failure mode % of failures
Engineering components
Aircraft components
Corrosion 29 16
Fatigue 25 55
Brittle fracture 16 -
Overload (ductile) 11 14
High temp. corrosion 07 02
SCC / Corrosion fatigue / HE
06 07
Creep 03 -
Wear/abrasion/erosion 03 06
June 28, 2012
![Page 12: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/12.jpg)
National Aerospace Laboratories
Fracture in metals
Ductile fracture
Ductile fracture involves gross plastic deformation and less catastrophic
Substantial energy is absorbed by microvoid coalescence (high energy fracture mode)
Brittle fracture
Brittle fracture does not involve gross plastic deformation and catastrophic
Low energy is absorbed during fracture (low energy fracture mode)
June 28, 2012
![Page 13: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/13.jpg)
National Aerospace Laboratories
Ductile fracture…macroscopic
Ductile fracture is less serious problem in engineering……plastic deformation
Under uniaxial tensile force, after necking, microvoids form and coalesce to form crack, which then propagate in the direction normal to the tensile axis
The crack then rapidly propagate through the periphery along the shear plane at 450 resulting in cup and cone fracture
June 28, 2012
![Page 14: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/14.jpg)
National Aerospace Laboratories
Ductile fracture…macroscopic
Microvoids are easily formed at inclusions, intermetallic or second phase particles and grain boundaries
June 28, 2012
![Page 15: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/15.jpg)
National Aerospace Laboratories
Ductile fracture…microscopic
Dimple rupture
June 28, 2012
![Page 16: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/16.jpg)
National Aerospace Laboratories
Ductile fracture…microscopic
Random planar array of particles acting as void initiators
Growth of voids to join each other as the applied stress increases
Linkage or coalescence of voids to form free fracture surface
June 28, 2012
![Page 17: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/17.jpg)
National Aerospace Laboratories
Ductile fracture…microscopic
2024 Al-alloy Steel
Decohesion at particle-matrix interface
Fracture of brittle particles
Decohesion of interfaces associated with shear deformation or grain boundary sliding
June 28, 2012
![Page 18: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/18.jpg)
National Aerospace Laboratories
Ductile fracture…microscopic
Tension
Torsion
June 28, 2012
![Page 19: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/19.jpg)
National Aerospace Laboratories
Ductile fracture…dimple shapes
FractographyASM Handbook
June 28, 2012
![Page 20: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/20.jpg)
National Aerospace Laboratories
Ductile fracture…microscopic
Structural steel Bearing steel
5 m
June 28, 2012
![Page 21: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/21.jpg)
National Aerospace Laboratories
Brittle fracture…macroscopic
Brittle fracture is a serious problem in engineering……no or negligible plastic deformation (catastrophic in nature)
Cleavage
Intergranular
Chevron marks
June 28, 2012
![Page 22: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/22.jpg)
National Aerospace Laboratories
Cleavage fracture……microscopic
Cleavage fracture surface is characterized by flat facets (size normally similar to grain size)
River lines or stress lines are steps between cleavage on parallel planes and always converge in the direction of local crack propagation
June 28, 2012
![Page 23: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/23.jpg)
National Aerospace Laboratories
Intergranular fracture……microscopic
Intergranular fracture is moderate to low energy brittle fracture mode resulting from grain boundary separation
Weak grain boundaries, grain boundary segregation, embrittlement
June 28, 2012
![Page 24: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/24.jpg)
National Aerospace Laboratories
Progressive fracture
Fatigue
Stress corrosion cracking (SCC)
Hydrogen embrittlement (HE)
Crack initiation followed by progressive
propagation over a period of time under fluctuating
load or sustained tensile load
June 28, 2012
![Page 25: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/25.jpg)
National Aerospace Laboratories
Progressive crack propagation(Crack arrest marks/beach marks) – can be fatigue or SCC or HE
Crack origin
Static overload failure
Progressive fracture……macroscopic
June 28, 2012
![Page 26: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/26.jpg)
National Aerospace Laboratories
Progressive fracture……crack origin
June 28, 2012
![Page 27: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/27.jpg)
National Aerospace Laboratories
Progressive fracture……crack origin
June 28, 2012
![Page 28: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/28.jpg)
National Aerospace Laboratories
Progressive fracture……crack origin
18.9 mm
12.4 mm
LE
Overload Fatigue
Differential exposure to
environment
June 28, 2012
![Page 29: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/29.jpg)
National Aerospace Laboratories
Progressive fracture……crack propagation direction
300 m30 m
Beach marks/clamshell marks
June 28, 2012
![Page 30: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/30.jpg)
National Aerospace Laboratories
Fatigue fracture……mechanisms
Stage I Propagation
Crack tends to grow initially along crystallographic planes of high shear stress: high stresses and notches tend to shorten this stage
It may propagate only over a few grains
Length of stage I is controlled by presence of stress raisers such as:
…………………
………………..
Stage II Crack growth rate increases (perpendicular to tensile stress direction)
Mostly transgranular crack propagation
Cracks that cause fatigue fracture almost always initiate/nucleate at component surface at some stress concentrations; scratches, dents, fillets, threads, weld beads/spatter………
June 28, 2012
![Page 31: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/31.jpg)
National Aerospace Laboratories
Fatigue fracture……mechanisms
Double notch at crack tip, extends along shear plane under tensile loading and then blunts due to deformation
Compression closes cracks and shear occurs in opposite sense leading to sharp notches again
And then again and again………………
The process leaves markings on the fracture surface; Beach Marks and/or Striations
Indicate position of crack tip at some point in time
June 28, 2012
![Page 32: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/32.jpg)
National Aerospace Laboratories
Fatigue fracture…… Foolproof signature
Stainless steel Hardened steel
June 28, 2012
![Page 33: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/33.jpg)
National Aerospace Laboratories
Fatigue fracture…… Foolproof signature
2024 Al-alloy Ti-6Al-4V
June 28, 2012
![Page 34: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/34.jpg)
National Aerospace Laboratories
Fatigue fracture……signatures
Ni-base superalloy (DS)
June 28, 2012
![Page 35: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/35.jpg)
National Aerospace Laboratories
Fatigue fracture……signatures
Ni-base superalloy (DS)
June 28, 2012
![Page 36: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/36.jpg)
National Aerospace Laboratories
Fatigue fracture……signatures
![Page 37: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/37.jpg)
National Aerospace Laboratories
Fatigue fracture……signatures
![Page 38: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/38.jpg)
National Aerospace Laboratories
Progressive fracture…… micro-mechanisms
Intergranular
(SCC, HE)
Crack initiation
Dimple rupture
Fatigue striations
Fatigue or SCC or HE????
June 28, 2012
![Page 39: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/39.jpg)
National Aerospace Laboratories
Conditions for SCC and HE cracking
A susceptible alloy
Aggressive environment
Applied or residual stress
A susceptible alloy
H2 in the material
Applied or residual stress
SCC HE
June 28, 2012
![Page 40: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/40.jpg)
National Aerospace Laboratories
SCC……mechanisms and prevention
Sources of Stress for SCC
Residual Applied
Welding
Shearing, Punching,Cutting
Bending, Crimping,Riveting
Machining(Lathe-Mill-Drill)
Heat Treating EDM, Laser/Wire Cutting
Grinding
Quenching Thermal Cycling Thermal Expansion Vibration Rotation Bolting Pressure
Dead Load
Stress Corrosion Cracking Triangle
Proper selection of material
Removing the corrosion species that promotes SCC
Change the manufacturing process or design to reduce the residual tensile stresses
Surface protection to avoid corrosion
June 28, 2012
![Page 41: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/41.jpg)
National Aerospace Laboratories
HE……mechanisms and prevention
Sources of hydrogen
Melting (generally causes blistering)
Environment (H2O during welding)
Surface treatment
Surface cleaning
Plating
……
Use material with lowest hardness in the specification range
Use clean steel (free of MnS inclusions…)
Baking as per the ASTM specification
Baking must be performed immediately after the processes where possibility of hydrogen pick up in the component exist
Hydrogen embrittlement Triangle
Hydrogen source
Sources of Stress for HE
Residual Applied
Welding
Shearing, Punching,Cutting
Bending, Crimping,Riveting
Machining(Lathe-Mill-Drill)
Heat Treating EDM, Laser/Wire Cutting
Grinding
Quenching Thermal Cycling Thermal Expansion Vibration Rotation Bolting Pressure
Dead Load
June 28, 2012
![Page 42: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/42.jpg)
National Aerospace Laboratories
SCC and HE…… How to distinguish?
SCC
HE
June 28, 2012
![Page 43: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/43.jpg)
National Aerospace Laboratories
SCC and HE…… How to distinguish?
SCC
HE
100m
Corrosion pit
June 28, 2012
![Page 44: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/44.jpg)
National Aerospace Laboratories
Applications
Case History I Inclusions_leading_to_fatigue.ppt
Case History II Corrosion_leading_to_fatigue.ppt
Case History III StressRupture_leading_to_fatigue.ppt
Case History IV Fretting_leading_to_fatigue.ppt
Case History V Hydrogen_embrittlement.ppt
Engineering Failure Analysis…
June 28, 2012
![Page 45: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/45.jpg)
National Aerospace Laboratories
Conclusions
Study of fracture surface provides information about how the material/component fractured
Behaviour of the material/component under service conditions
Mandatory for engineering failure analysis
Research in materials science
Fracture-path studies
Deformation before and during fracture
Fracture-surface characteristics
Estimation of grain size
Weak micro constituents etc
Many more…………………
June 28, 2012
![Page 46: Fractography: The Way Things Fracture - ERNETmaterials.iisc.ernet.in/~ugc/nrcmmpc12/Fractography_IISc_28062012.pdf · applied stress increases ... Modern physical metallurgy & materials](https://reader031.vdocuments.net/reader031/viewer/2022022516/5b02622e7f8b9a54578f9d02/html5/thumbnails/46.jpg)
National Aerospace Laboratories
Suggested Reading
G.E. Dieter, Mechanical metallurgy, 1988, SI metric edition, McGraw-Hill, ISBN 0-07-100406-8
R.J. Sanford, Principles of fracture mechanics, 2003, Prentice Hall, ISBN 0-13-192992-1
Fractography, Vol.12, eighth edition, ASM Handbook, ASM International, 1987
R.E. Smallman, R.J. Bishop, Modern physical metallurgy & materials engineering, 1999, sixth edition, Butterworth-Heinemann, ISBN 0-7 506-4564-4
A.H. Cottrell, Theory of Brittle Fracture in steel and similar metals, 1958, Transactions of the metallurgical society of AIME, Vol.212, p. 192-203
Failure analysis and prevention, Vol.11, ASM Handbook, ASM International, 2002
June 28, 2012