libro cuaderno de metalografÍa
TRANSCRIPT
![Page 1: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/1.jpg)
CUADERNO DE DIBUJOS METALOGRÁFICOS DE LOS ALUMNOS DE LA LICENCIATURA EN CIENCIAS QUÍMICAS
Antonio J. Criado Portal
![Page 2: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/2.jpg)
2
““““CUADERNO DE DIBUJOS METALOGRAFICOS CUADERNO DE DIBUJOS METALOGRAFICOS CUADERNO DE DIBUJOS METALOGRAFICOS CUADERNO DE DIBUJOS METALOGRAFICOS
DE LOS ALUMNOS DE LA LICENCIATURA EN DE LOS ALUMNOS DE LA LICENCIATURA EN DE LOS ALUMNOS DE LA LICENCIATURA EN DE LOS ALUMNOS DE LA LICENCIATURA EN
CIENCIAS QUÍMICASCIENCIAS QUÍMICASCIENCIAS QUÍMICASCIENCIAS QUÍMICAS”
por
Antonio J. Criado Portal
Profesor Titular del Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica. Facultad de Ciencias Químicas. Universidad Complutense de Madrid. 28040 MADRID.
Madrid, Abril de 2012
Editor científico: Antonio J. Criado Portal.
![Page 3: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/3.jpg)
3
A mis alumnos de metalografía
![Page 4: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/4.jpg)
4
Índice Página
I. INTRODUCCIÓN
5
II. LISTADO DE MICROESTRUCTURAS
METALOGRÁFICAS
7
III. ÁLBUM METALOGRÁFICO
8
IV. DIBUJOS DE AUTOR
80
V. BIBLIOGRAFÍA
112
![Page 5: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/5.jpg)
5
I. INTRODUCCIÓN
Llevo muchos años enseñando metalografía en este Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica de la Universidad Complutense de Madrid. Pienso que esta técnica de análisis de estructuras es fundamental para el conocimiento e interpretación de las características mecánicas y fisicoquímicas de los materiales metálicos. Para su utilización requiere de buenos conocimientos científicos y tecnológicos sobre los metales y sus aleaciones, además de unas buenas dosis del arte de interpretar imágenes. La metalografía es, básicamente, interpretación de imágenes, claro está, ajustándose a las reglas derivadas de la ciencia y tecnología metalúrgica.
El conocimiento de los diagramas de equilibrio es fundamental para la
interpretación correcta de lo observado a través del microscopio. Como es natural, otras técnicas científicas auxiliares, participan en la ayuda a la identificación de fases y microconstituyentes: Difracción de rayos-X, análisis EDS-EDX, etc. Pero no demos mayor importancia a lo que no lo tiene. La metalografía exige de una buena dosis de imaginación y visión de las formas geométricas observadas para situarse ante la solución de un problema. Las otras técnicas, certifican nuestro diagnóstico inicial. Si no se intuye, a través de las imágenes observadas, la solución, el resto de técnicas auxiliares sólo servirán para embrollar aún más el problema. La Naturaleza es muy simple y siempre resuelve las más diversas situaciones con soluciones sencillas. Es absurdo utilizar la metalografía para esconder el desconocimiento de una solución sencilla, a la que no se es capaz de llegar.
Mis alumnos me han demostrado, a lo largo de muchos años, su capacidad de
observación. Y no es fácil para un principiante asomarse al “tubo” y ver “algo”. Sin embargo, inculcándoles conocimientos simples y precisos, y una generosa dosis de imaginación, los resultados son sorprendentes.
En este cuaderno presento algunos de los dibujos realizados por mis alumnos, de
estructuras metalográficas observadas con el microscopio óptico y discutidas en la clase. Sólo os presento algunos ejemplos a modo de botón de muestra. Ninguno ha hecho Bellas Artes, pero poseen el arte natural de los que se toman las imágenes observadas como un reflejo de algo más allá de lo que se puede intuir. En algunos casos el dibujo posee grandes dosis de ingenuidad. En otras ocasiones, son de un realismo asombroso.
El material utilizado para estos magníficos dibujos metalográficos es elemental:
lápices de colores, rotuladores, bolígrafos, goma,…., y una cuartilla, muchas veces cuadriculada.
El arte y la creación pueden, en numerosas ocasiones, prescindir de materiales
nobles para su realización. Estos dibujos, muchas veces obtenidos de la misma imagen observada, son creaciones personales.
No he utilizado todo el material producido, he elegido algunas estructuras
metalográficas muy clásicas y los correspondientes dibujos de mis queridos artistas. Estos dibujos han sido fotografiados y expuestos en toda su creatividad original. No figuran los aumentos para no estropear la estética de los dibujos.
![Page 6: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/6.jpg)
6
Las imágenes que se presentan en el álbum son fotografías obtenidas directamente de los dibujos, sin ningún tipo de retoque para no desvirtuar tono, contraste, colorido,…, del original.
![Page 7: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/7.jpg)
7
II. LISTADO DE MICROESTRUCTURAS METALOGRÁFICAS
1. ESTRUCTURA DE COLADA (granos columnares) 2. ESTRUCTURA DEL EUTÉCTICO Al-Zn
3. ESTRUCTURA DEL PERITÉCTICO Sn-Sb
4. ESTRUCTURA DE LA ALEACIÓN Cu-P EUTÉCTICA E
HIPEREUTÉCTICA.
5. ESTRUCTURA DE LA ALEACIÓN Cu-P HIPOEUTÉCTICA (microsegregación)
6. ESTRUCTURA DE UN SIDERITO
7. ESTRUCTURA WIDMANSTÄTTEN DE LA ALEACIÓN Ti-Al
8. ESTRUCTURA DE MOLDEO DEL LATÓN Cu-42Zn
9. ESTRUCTURA DE LA ALEACIÓN Al-4Cu (moldeada, templada, y templada
y revenida)
10. ESTRUCTURA DE ACERO EUTECTOIDE LAMINADO EN CALIENTE Y NORMALIZADO
11. ESTRUCTURA DE ACERO HIPOEUTECTOIDE LAMINADO EN
CALIENTE Y NORMALIZADO
12. ESTRUCTURA DE ACERO HIPEREUTECTOIDE LAMINADO EN CALIENTE Y NORMALIZADO
13. ESTRUCTURA DE ACERO CEMENTADO Y ESTRUCTURA DE COLADA
DE ACERO HIPOEUTECTOIDE
14. ESTRUCTURA DE MOLDEO DEL ACERO AL CRISOL (A. Damasco)
15. ESTRUCTURA DE ACERO DE DAMASCO FORJADO
16. ESTRUCTURA CON PERLITA FINA, MARTENSITA Y AUSTENITA REVENIDA
17. ESTRUCTURA DE BAINITA Y MARTENSITA REVENIDA
18. ESTRUCTURA DE ACERO ALEADO AUSTENÍTICO (Hadfield)
19. ESTRUCTURA DE PUÑAL CELTA FABRICADO EN EL LABORATORIO
DE TECNOLOGÍA MECÁNICA DE LA UNIVERSIDAD COMPLUTENSE DE MADRID
![Page 8: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/8.jpg)
8
III. ÁLBUM METALOGRÁFICO
1. ESTRUCTURA DE COLADA (granos columnares)
![Page 9: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/9.jpg)
9
![Page 10: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/10.jpg)
10
![Page 11: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/11.jpg)
11
2. ESTRUCTURA DEL EUTÉCTICO Al-Zn
![Page 12: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/12.jpg)
12
![Page 13: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/13.jpg)
13
![Page 14: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/14.jpg)
14
3. ESTRUCTURA DEL PERITÉCTICO Sn-Sb
![Page 15: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/15.jpg)
15
![Page 16: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/16.jpg)
16
![Page 17: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/17.jpg)
17
4. ESTRUCTURA DE LA ALEACIÓN Cu-P EUTÉCTICA E HIPEREUTÉCTICA
![Page 18: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/18.jpg)
18
![Page 19: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/19.jpg)
19
5. ESTRUCTURA DE LA ALEACIÓN Cu-P HIPOEUTÉCTICA (microsegregación)
![Page 20: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/20.jpg)
20
![Page 21: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/21.jpg)
21
![Page 22: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/22.jpg)
22
![Page 23: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/23.jpg)
23
![Page 24: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/24.jpg)
24
![Page 25: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/25.jpg)
25
6. ESTRUCTURA DE UN SIDERITO
![Page 26: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/26.jpg)
26
![Page 27: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/27.jpg)
27
![Page 28: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/28.jpg)
28
7. ESTRUCTURA WIDMANSTÄTTEN DE LA LAEACIÓN Ti-Al
![Page 29: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/29.jpg)
29
![Page 30: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/30.jpg)
30
![Page 31: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/31.jpg)
31
![Page 32: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/32.jpg)
32
8. ESTRUCTURA DE MOLDEO DEL LATÓN Cu-42Zn
![Page 33: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/33.jpg)
33
![Page 34: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/34.jpg)
34
![Page 35: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/35.jpg)
35
9. ESTRUCTURA DE LA ALEACIÓN Al-4Cu (moldeada, templada, y templada y revenida)
![Page 36: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/36.jpg)
36
![Page 37: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/37.jpg)
37
![Page 38: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/38.jpg)
38
![Page 39: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/39.jpg)
39
![Page 40: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/40.jpg)
40
10. ESTRUCTURA DE ACERO EUTECTOIDE LAMINADO EN CALIENTE Y NORMALIZADO
![Page 41: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/41.jpg)
41
![Page 42: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/42.jpg)
42
11. ESTRUCTURA DE ACERO HIPOEUTECTOIDE LAMINADO EN CALIENTE Y NORMALIZADO
![Page 43: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/43.jpg)
43
![Page 44: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/44.jpg)
44
![Page 45: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/45.jpg)
45
![Page 46: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/46.jpg)
46
![Page 47: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/47.jpg)
47
![Page 48: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/48.jpg)
48
![Page 49: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/49.jpg)
49
12. ESTRUCTURA DE ACERO HIPEREUTECTOIDE LAMINADO EN CALIENTE Y NORMALIZADO
![Page 50: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/50.jpg)
50
![Page 51: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/51.jpg)
51
![Page 52: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/52.jpg)
52
![Page 53: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/53.jpg)
53
![Page 54: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/54.jpg)
54
![Page 55: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/55.jpg)
55
![Page 56: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/56.jpg)
56
13. ESTRUCTURA DE ACERO CEMENTADO Y ESTRUCTURA DE COLADA DE ACERO HIPOEUTECTOIDE
![Page 57: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/57.jpg)
57
![Page 58: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/58.jpg)
58
14. ESTRUCTURA DE MOLDEO DEL ACERO AL CRISOL (A. Damasco)
![Page 59: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/59.jpg)
59
![Page 60: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/60.jpg)
60
![Page 61: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/61.jpg)
61
![Page 62: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/62.jpg)
62
15. ESTRUCTURA DE ACERO DE DAMASCO FORJADO
![Page 63: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/63.jpg)
63
![Page 64: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/64.jpg)
64
![Page 65: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/65.jpg)
65
![Page 66: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/66.jpg)
66
16. ESTRUCTURA CON PERLITA FINA, MARTENSITA Y AUSTENITA REVENIDA
![Page 67: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/67.jpg)
67
![Page 68: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/68.jpg)
68
![Page 69: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/69.jpg)
69
![Page 70: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/70.jpg)
70
17. ESTRUCTURA DE BAINITA Y MARTENSITA REVENIDA
![Page 71: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/71.jpg)
71
![Page 72: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/72.jpg)
72
![Page 73: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/73.jpg)
73
18. ESTRUCTURA DE ACERO ALEADO AUSTENÍTICO (Hadfield)
![Page 74: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/74.jpg)
74
![Page 75: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/75.jpg)
75
![Page 76: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/76.jpg)
76
19. ESTRUCTURA DE PUÑAL CELTA FABRICADO EN EL LABORATORIO DE TECNOLOGÍA MECÁNICA DE LA UNIVERSIDAD COMPLUTENSE DE MADRID
![Page 77: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/77.jpg)
77
![Page 78: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/78.jpg)
78
![Page 79: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/79.jpg)
79
![Page 80: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/80.jpg)
80
IV. DIBUJOS DE AUTOR
• ALEJANDRA SANCHEZ-BAYO ÁLVAREZ.
Acero de Damasco forjado.
Acero hipereutectoide.
![Page 81: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/81.jpg)
81
Acero hipoeutectoide.
Bronce de fósforo hipoeutéctico.
![Page 82: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/82.jpg)
82
Perlita fina.
Puñal celta.
![Page 83: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/83.jpg)
83
• ARANTZAZU CASERO PERPIÑA.
Acero De Damasco forjado.
Acero hipereutectoide.
![Page 84: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/84.jpg)
84
Acero hipoeutectoide.
Aleación Sn-Sb.
![Page 85: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/85.jpg)
85
Bronce de fósforo hipoeutéctico.
Dural envejecido.
![Page 86: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/86.jpg)
86
Latón bifásico.
Microrrechupes en un bronce.
![Page 87: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/87.jpg)
87
Perlita Fina.
Soldadura fuerte con cobre.
![Page 88: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/88.jpg)
88
• AURORA GÓMEZ BLANCO.
Acero de Damasco forjado.
Acero hipereutectoide.
![Page 89: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/89.jpg)
89
Acero hipoeutectoide.
Aleación Sn-Sb.
![Page 90: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/90.jpg)
90
Dural envejecido.
Latón bifásico.
![Page 91: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/91.jpg)
91
Puñal celta.
Soldadura fuerte con cobre.
![Page 92: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/92.jpg)
92
• FERNANDO SERRANÍA ALARCÓN.
Acero de Damasco forjado.
Acero hipereutectoide.
![Page 93: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/93.jpg)
93
Acero hipoeutectoide.
Aleación Sn-Sb.
![Page 94: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/94.jpg)
94
Bronce de fósforo hipoeutéctico.
Dural envejecido.
![Page 95: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/95.jpg)
95
Estructura de colada.
Latón bifásico.
![Page 96: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/96.jpg)
96
Microrrechupes en un bronce.
Perlita fina.
![Page 97: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/97.jpg)
97
Puñal celta.
Soldadura fuerte con cobre.
![Page 98: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/98.jpg)
98
• MATILDE SAURA MUZQUIZ.
Estructura de colada (F. Calvo).
![Page 99: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/99.jpg)
99
Microrrechupes en un bronce ( F. Calvo).
![Page 100: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/100.jpg)
100
Aleación Cu-P hipoeutéctica sin ataque (F. Calvo).
![Page 101: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/101.jpg)
101
Aleación Sn- Sb (F. Calvo).
![Page 102: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/102.jpg)
102
Latón bifásico (F. Calvo).
![Page 103: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/103.jpg)
103
Dural envejecido (F. Calvo).
![Page 104: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/104.jpg)
104
Acero hipereutectoide (F. Calvo).
![Page 105: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/105.jpg)
105
Soldadura fuerte con cobre (F. Calvo).
![Page 106: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/106.jpg)
106
Puñal celta.
![Page 107: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/107.jpg)
107
• PAULA MORA AYUSO.
Acero de Damasco forjado.
Acero hipereutectoide.
![Page 108: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/108.jpg)
108
Acero hipoeutectoide.
Aleación Cu-P hipoeutéctica. .
![Page 109: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/109.jpg)
109
Aleación Sn-Sb.
Dural envejecido.
![Page 110: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/110.jpg)
110
Estructura de colada.
Latón bifásico.
![Page 111: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/111.jpg)
111
Microrrechupes en un bronce.
![Page 112: LIBRO CUADERNO DE METALOGRAFÍA](https://reader036.vdocuments.net/reader036/viewer/2022082217/58736a011a28abab268b7c5a/html5/thumbnails/112.jpg)
112
V. BIBLIOGRAFÍA
- F. A. Calvo: “Metalografía Práctica”. Editorial Alambra. Madrid, 1971.
- C. S. Smith: “A History of Metallography”. The University Chicago Press. Chicago, 1960.
- G. A. Chadwick: “Metallography of Phase TRansformations”.
Butterworth & Co Ltd. London, 1972.
- A. J. Criado: “Estructuras Metalográficas de Aleaciones Hierro-Carbono: Aceros al Carbono y Fundiciones”. Edición on-line: www.antoniocriado.es. Madrid, 2008.
- A. J. Criado: “Estructuras Metalográficas de los Aceros Especiales”.
Edición on-line: www.antoniocriado.es. Madrid, 2010.