moulding defects 1.pdf
TRANSCRIPT
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 1/158
1
MOULDING DEFECTSAND
REMEDIES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 2/158
2
~ HOW MANY KINDS OF DEFECTS ARE THERE?
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 3/158
3
~ HOW MANY KINDS OF DEFECTS ARE
THERE?
31
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 4/158
4
DEFECTS
1. Sink Marks
2. Streaks
3. Blistering
4. Weld Lines
5. Gloss difference
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 5/158
5
6. Jetting
7. Record grooves effect
8. Dull spots near gate area
9. Incompletely filled part ( Shortshots)
10. Diesel effect
DEFECTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 6/158
6
11.Over sprayed parts (Flashes)
12.Stress whitening/Cracking
13.Ejector marks
14.Deformation during demolding
15. Ejection Grooves
DEFECTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 7/158
7
DEFECTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 8/158
8
21. Defects on electroplated parts
22. Broken or ragged film hinge
23. Warpage24. Fish eye
DEFECTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 9/158
9
25. Hesitation
26.Over packing
27. Unbalanced flow
DEFECTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 10/158
10
28. Nozzle drool
29. Nozzle freeze – off
30 Nozzle spitting31. Screw slip
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 11/158
11
WHAT ARE THE MAIN FACTORS
CAUSING DEFECTS?
4M?
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 12/158
12
SOME MAIN FACTORS CAUSING DEFECTS
The moulding Machine
Mould
Operating conditions i.e..Temperature, pressure, injectionspeed & time
Material. Design of product
Management
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 13/158
13
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 14/158
14
!!"
!"#$%&#
SINKMARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 15/158
15
!"#$%&#
SINK
MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 16/158
16
!"#$%&#
SINK MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 17/158
17
Sink marks on a cylindrical core with poor
temperature control
Sinkmarks
!"#$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 18/158
18
Sink marks appear as depressions on the surfaceof a molded part.
These depressions are typically very small;
however they are often quite visible, because theyreflect light in different directions to the part.
!"#$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 19/158
19
CAUSE OF SINK MARKS
Sink marks occur during the cooling process ifcertain areas of the part are not cooled
sufficiently causing them to contract
If these contractions are not compensated andthe outside wall is not stable enough due toinsufficient cooling depressions occur
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 20/158
20
!!!"#
$ %&%&$ '($ )&"
$ '(
*+,
-+'!!"
.+/
%'%(%)*&*!"#$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 21/158
21
Disadvantageous Gating
Moulded part with sink marks
(Gating at the thin wall)
Solidified Peripheral
!"#$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 22/158
22
0+ "&
*+ "
-+ !&""1("
*!+(,*(')!*"*&!"#$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 23/158
23
.+ '2+!(3!"(
4+ 3
*!+(,*(')!*"*&!"#$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 24/158
24
2. STREAKS
Streaks are the prominent stretchy markson the surface of the moldings.
CHARRED STREAKS
MOISTURE STREAKS
AIR STREAKS
COLORED STREAKS
GLASS FIBER STREAKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 25/158
25
Charred streaks due to excessive residence time in
the plasticising cylinder
2.CHARRED STREAKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 26/158
26
Streaks due to excessive moisture content of thegranules
2.MOISTURE STREAKS:
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 27/158
27
&
2.AIR STREAKS:
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 28/158
28
&5!!
2.COLOUR STREAKS:
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 29/158
29
&&
2.COLOUR STREAKS:
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 30/158
30
/!&631&(7
-(%!+&,)&,%#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 31/158
31
"""3"
"
""
!!53"!"
%'%(%)*&*&)&,%#
%'%( %)*& *& )&,%#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 32/158
32
""!
!"(
,1"
%'%(%)*&*&)&,%#
*!+(, *(')!*" *& )&,%#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 33/158
33
0+ !&1""
3%(%3
*+ !"3+
*!+(,*(')!*"*&)&,%#
*!+(, *(')!*" *& )&,%#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 34/158
34
-+ !&"'1%""
.+ &!!3
4+ """
*!+(,*(')!*"*&)&,%#
*!+(, *(')!*" *& )&,%#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 35/158
35
6. Reduce residence time in material hopper
7. Reduce injection rate
8. Round sharp edges of transitions.
9. Reduce depth of engraving
10. Provide for venting
*!+(,*(')!*"*&)&,%#
*!+(, *(')!*" *& )&,%#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 36/158
36
11. Use smaller colour pigments
12. Check solubility of the used die
13. Use shorter glass fiber
*!+(,*(')!*"*&)&,%#
3.BLISTERS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 37/158
37
3.BLISTERS
0+ &&&!(!(
AIR BUBBLES
Hollows created on or in the molded part
3.BLISTERS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 38/158
38
Air traps occur when converging flow frontssurround and trap a bubble of air.
The trapped air can cause
Incomplete filling and packing, Surface blemish in the final part. Air trapped in pockets may compress, heat up
and cause burn marks.
3.BLISTERS
3.BLISTERS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 39/158
39
3.BLISTERS
(hollows created on or in the molded part)
*+8(+
voids
3.BLISTERS / BUBBLES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 40/158
403.Bubbles
Bubbles
3.BLISTERS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 41/158
41
4.Blisters and delamination
DELAMINATION
%'%( %)*& *& +(!),&
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 42/158
42
913"!
!!3
8"&
"
%'%(%)*&*&+(!),&
*!+(,*(')!*"*&+(!),&
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 43/158
43
0+
*+ (
-+ 3
.+ &
* * ' * *
*!+(,*(')!*"*&+(!),&
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 44/158
44
4+
:+ "
;+ ,11
<+ "
4 WELD LINE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 45/158
45
4.WELD LINE
(Witness marks of two or more melt flow fronts at their joining
zone)
=((!(!&3"31&+
(!
3(!
WELD LINE
%'%(%)*&*.,((!",
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 46/158
46
=( '(
91& 1" =( '13( !"(&"
,!(
*!+(,*(')!*"*&.,((!",
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 47/158
47
0+ '
*+ '
-+ '
.+ 2
*!+(,*(')!*"*&.,((!",
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 48/158
48
4+ 15
:+ 813(
;+ 1"61(1&
7
<+ 1!(
5.GLOSS/GLOSS DIFFERENCES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 49/158
49
Very glossy impression due to reflection on the polished surface
5.GLOSS/GLOSS DIFFERENCES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 50/158
50
Only slightly glossy impression due to reflection on a roughsurface
5 GLOSS/GLOSS DIFFERENCES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 51/158
51
5.GLOSS/GLOSS DIFFERENCES
"!!"3!!(9"+
3!"!("6!7+
!!"""!!"3"
!""+
5.GLOSS/GLOSS DIFFERENCES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 52/158
52
5.GLOSS/GLOSS DIFFERENCES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 53/158
53
%'%(%)*&*&-(*!,&,",
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 54/158
54
!!"
"!!
"!3+"+("
9!
,!
*!+(,*(')!*"*&-(*!,&,",
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 55/158
55
0+ !
*+ !"(!"!
-+
.+ 1">
6.JETTING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 56/158
56
The prominent inhomogeneous snake like strandson the surface of molding
?""""%"1+
JETTINGJETTING
/,))!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 57/158
57
!3'("'
"!(!
1 ! &
Mould filling process in frontal flow and with jetting
/,))!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 58/158
58THREE EXAMPLE OF JETTING
6.JETTING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 59/158
59
Jetting occurs when polymer melt is pushed at a highvelocity through restrictive areas, such as the nozzle,runner, or gate, into open, thicker areas, without formingcontact with the mold wall. Jetting leads to part weakness,surface blemishes, and a multiplicity of internal defects.
*!+(,*(')!*"*&/,))!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 60/158
60
0+ '
*+ "%(
-+ "
.+ 1"(!13&&(
7.RECORD GROOVES EFFECT
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 61/158
61
83!"1!!
#
0+ !!2
*+ '
7.RECORD GROOVES EFFECT
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 62/158
62
RECORD GROOVE OR ORANGE PEEL
*!+(,*(')!*"*&&,*&-&**0,,,)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 63/158
63
0+
*+ +
-+ 1
.+ '
4+ 9'
8.DULL SPOTS IN GATE AREA
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 64/158
64
"3&3
0+ "*+ "'+
'((*)!"-%),%&,%
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 65/158
65
!(+
"'"&3"!"'+
"!93&"3!(3"3+
'((*)!"-%),%&,%
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 66/158
66
!(+
3&(13""!"+
!(((!
93!+
(3!
*!+(,*(')!*"*&'((*)!"-%),%&,%
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 67/158
67
0+ '
*+ "
-+ !!"13
.+ 1!"
9.INCOMPLETELY FILLED PART (SHORT SHOTS)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 68/158
68
!1!3+
SHORT SHOT
9.INCOMPLETELY FILLED PART (SHORT SHOTS)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 69/158
69
INCOMP0LETELYFILLED
9.INCOMPLETELY FILLED PART (SHORT SHOTS)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 70/158
70
A short shot is the incomplete filling of a mold cavitywhich results in the production of an incomplete part.
The flow freezes off before all of the flow paths havefilled.
%'%(%)*&*&1*&)1*)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 71/158
71
'1617
,1"
'!!
"
%'%(%)*&*&1*&)1*)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 72/158
72
(%!
3!1&!(
&!!(
13
!!""
*!+(,*(')!*"*&1*&)1*)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 73/158
73
0+ '%
*+
-+ +!1
.+ !
*!+(,*(')!*"*&1*&)1*)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 74/158
74
4+131+
:+!511"913
;+""+
!3!3%3@!%"&&113(+!"(%"
1
10.DIESEL EFFECT / BURNED MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 75/158
75
!!!!(2
1&+
A"(!&3"
3&31&+
BURNED MARKS
10.DIESEL EFFECT / BURNED MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 76/158
76BURN MARKS
BURN MARKS
10.DIESEL EFFECT / BURNED MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 77/158
77
BURNS
BURNS
10.DIESEL EFFECT / BURNED MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 78/158
78
31"&%"""""&+
&%!%(&%(1!(!%!
!(+
0+ "B"
*!+(,*(')!*"*& !,,(,,)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 79/158
79
" "
*+ '
-+ '
.+ B
4+ 1131"+
83&1(3(&&"&"
11.FLASHES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 80/158
80
!"!%!1"1%('+
!((&+
>1,C
FLASHES
11.FLASHES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 81/158
81
Flashing occurs when a thin layer of material is
11.FLASHES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 82/158
82
forced out of the mold cavity at the parting line orejector pins location.
This excess material remains attached to themolded article, and normally has to be manuallyremoved.
11.FLASHES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 83/158
83
FLASHES
%'%(%)*&*&(%1,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 84/158
84
,&"(9%!!"%9"%""!
"!"(
"
!!13!
*!+(,*(')!*"*&(%1,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 85/158
85
0+
*+ 1"+831&"!&"
-+ "!3!!3&3D&"E"
*!+(,*(')!*"*&(%1,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 86/158
86
.+ '&+
4+ 3&"("!("+
:+ 3&"!&"(1+
12.STRESS WHITENING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 87/158
87
""&3"
&39!+
3&&3&
9&"!
!F3
(!1&+
12.STRESS WHITENING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 88/158
88STRESS WHITENING
*!+(,*(')!*"*&)&,.1!),"!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 89/158
89
0+ '
*+ 3
-+ 3
.+
*!+(,*(')!*"*&)&,.1!),"!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 90/158
90
4+
:+ !3'
;+ !333B
<+ !3B
13.EJECTOR MARKS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 91/158
91
'1"&"(3!
!!+
DEPRESSED EJECTORMARKS
%',*&,/,)*&$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 92/158
92
"""!
"!!(&(('
,"""!
"!"'"
*!+(,*(')!*"*&,/,)*&$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 93/158
93
0+ &!!'
*+ !'
-+ "'"3
.+ "
*!+(,*(')!*"*&,/,)*&$%&#
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 94/158
94
4+ "'3
:+ !
;+ "!!"%"
14.DEFORMATION DURING DEMOULDING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 95/158
95
&(3""+
3&&+
DEFORMATION ON THE MOULDED PART DUE TO FORCED DE MOULDING
DEFORMATION
*!+(,*(')!*"*&,*&$%)!*"'&!"-,$*'(!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 96/158
96
0+ "
*+ "
-+ "
.+ '
*!+(,*(')!*"*&,*&$%)!*"'&!"-,$*'(!"-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 97/158
97
4+ )!3"!
:+ !"!"
;+)"
15.EJECTION GROOVES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 98/158
98
'"1""
"!!+
33!+
3
%',*&,/,)!*"-&**0,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 99/158
99
3
=!+
!"+
!9113+
!!+
*!+(,*(')!*"*&,/,)!*"-&**0,
0+ "
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 100/158
100
0+ "
*+ (
-+ !
.+ )(!"
4+ !!
16.FLAKING OF SURFACE LAYER
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 101/158
101
("!3!"!!!!
&"&('3+
FLAKING
0+ ! + &
*!+(,*(')!*"*&(%#!"-*'&%,(%2,&
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 102/158
102
0+ !+&31&39"
&
*+ 3
-+
.+
4+ !!A"+"3"!
17.COLD SLUG
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 103/158
103 "!(!
"&!13!+
COLD SLUG NEAR THE GATE
17.COLD SLUG
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 104/158
104 "!(!
"&!13!+
WELD LINE BEHIND A COLD SLUG
17.COLD SLUG
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 105/158
105 "!(!
"&!13!+
FLOW FRONT TRANSFORT THE COLD SLUG IN TO THE MOULD
%',*&*(('-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 106/158
106
3&
!
"&&
,&
%',*&*(('-
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 107/158
107
,&
0+ "
*+ "3
-+
.+ 1'&(
18.FILAMENTATION
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 108/158
108
!!"!"%&3!"+
3"!!!1+
"3(
!!!!+
Long filamentation of a cold runner gating system near the machinenozzle
18.FILAMENTATION
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 109/158
109
!!"!"%&3!"+
3"!!!1+
"3(
!!!!+
Long filament near a hot runner gate
0 , !!
*!+(,*(')!*"*&!(%$,")%)!*"
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 110/158
110
0+ ,1!!""3+
*+ 91"+
-+
!!+
.+ ""+
*!+(,*(')!*"*&!(%$,")%)!*"
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 111/158
111
" "
4+ 31&&!("+
:+ +
;+ "
19.DARK SPOTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 112/158
112
&&(&"31+
3&
1"!!"%(1"+
19.DARK SPOTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 113/158
113Severe black specks
19.DARK SPOTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 114/158
114
Poor screw flights design ,dead spots lead to black specks
#%"%
%',*&%&#*)
&
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 115/158
115
,&
0+ !!+
*+ &+
-+ +
.+ +
#%"%
%',*&%&#*)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 116/158
116
,&
$ 15+
$ ,11+
$ ,""3+
$ 13+
20.PLATE OUT
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 117/158
117
,!!!+"(13!!1+
3,%,,%,A%,%,)%,(1!%&
&'
ROUGH SURFACE DUE TO PLATE OUT IN THE MOULD
20.PLATE OUT
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 118/158
118
PLATE OUT NEAR THE GATE
,!!!+"(13!!1+
3,%,,%,A%,%,)%,(1!%&&'
"91!&
%',*&(%),*')
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 119/158
119
&3!%&&+
3""+
"%91%%+
0+ )&&
*!+(,*(')!*"*&(%),*')
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 120/158
120
*+ "!&+
-+ )!3!1"+
.+ &3!&(1BB&+
4+ 9"+
*!+(,*(')!*"*&(%),*')
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 121/158
121
:+
;+ !!1"+
<+
21.DEFECTS ON ELECTROPLATED PARTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 122/158
122
!6%&%!!37+
!'1&+
!(
"+
PIMPLES AND BLISTERS ON A MOULDED PART
21.DEFECTS ON ELECTROPLATED PARTS
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 123/158
123
!6%&%!!37+
!'1&+
!(
"+
BLISTERING DUE TO DRAWN –IN AIR (COMPONENTWITH AND WITHOUT ELECTROLITIC LAYER)
*!+(,*(')!*",,)*",(,)&*(%),%&)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 124/158
124
0+ '
*+ (("+
-+ +
.
*!+(,*(')!*",,)*",(,)&*(%),%&)
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 125/158
125
.+ 1(1+
4+ 1!"
:+ 1+
;+ ""+
22.BROKEN/ RAGGED FILM HINGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 126/158
126
"1"'+
!&!+
STRESS WHITENING ON A FILM HINGE
22.BROKEN/ RAGGED FILM HINGE
STREE
WHITENING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 127/158
127
!!!"3&3
13+ !"3&33+
1"("+
STRESS WHITENING ON A FILM HINGE
!!!
0+ +
*!+(,*(')!*"*&+&*#,"3&%--,!($1!"-,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 128/158
128
0+ +
*+ '+
-+ (+
.+ (!!"+
4+ )!(
:+ 1!""(3!"+
*!+(,*(')!*"*&+&*#,"3&%--,!($1!"-,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 129/158
129
!!>"+
0+ (
*+ )!(!3
-+ ""
!&3!!(+
*!+(,*(')!*"*&+&*#,"3&%--,!($1!"-,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 130/158
130
3
0+ 1(!!"+
*+ (+
-+ )!"13
.+ !(!!(!
23.WARPAGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 131/158
131
"1!!>+
"%,(&"&(%(%&(&3!("
MOULDED PART WITH WARPAGE ON THE EDGE
23.WARPAGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 132/158
132
"1!!>+
"%,(&"&(%(%&(&3!("
WARPAGE IN THE FLANGE AREA
WARPAGE
23.WARPAGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 133/158
133
Variation in mould temperature will cause
component to warp
23.WARPAGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 134/158
134
Warped component
23. WARPAGE
Distortion of the part caused by non-uniform shrinkage of
the plastic.
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 135/158
135
23.WARPAGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 136/158
136
Typical warpage in most radiator end tanks.
Article ejected too hot.
Variation in section thickness or contours of the
%'%(%)*&*&.%&%-,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 137/158
137
a at o sect o t c ess o co tou s o t escrew.
Excessive area discharged or packed into the areaaround the gate.
Non-uniform mould temperature due to improperpositioning if the cooling channels in the mould.
Excessive feed.
'"+
CAUSAL FACTORS FOR WARPAGE
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 138/158
138
!!"+
,3""3+
)&"("+
"+
*!+(,*(')!*"*&.%&%-,
0+ '615%11"7+%
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 139/158
139
"711"7+%
11"7+
*+ "!>+
-+ !"+
.+ >B&!&1+
*!+(,*(')!*"*&.%&%-,
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 140/158
140
4+ '5+
:+ "+
;+ "&+
<+ 3""'+
Fish eyes are a surface defect that results fromun melted material being pushed with the meltstream into the cavity and appearing on the surface
24. FISH EYES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 141/158
141
y pp gof a molded part.
Remedies for Fish eyes
1. Reduce regrind materialC i l li h d d
24. FISH EYES
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 142/158
142
Contact material suppliers to get the recommended
levels of regrind to use.
2. Optimize melt temperature
3. Modify screw designContact material suppliers to get the right screw
design information to avoid improper melt mix oroverheating that leads to material degradation.
Hesitation is when flow slows down or stops along
a particular flow path. If plastic filling a cavity has the option of filling either
a thin section or a thick section the plastic will tend
25. HESITATION
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 143/158
143
a thin section or a thick section, the plastic will tend
to fill the thick section first as this route offers lessresistance to flow.
Hesitation can occur in ribs and in thin section ofparts that have significant changes in wallthickness.
25. HESITATION
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 144/158
144
Remedies for Hesitation
1. Move the polymer injection location away fromh f h i i h h b lk f h
25. HESITATION
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 145/158
145
the area of hesitation so that the bulk of the
cavity fills before the melt reaches the thin area.
2. Move the polymer injection location to a place
that will cause greater pressure to be appliedwhere the hesitation occurred.
Remedies for Hesitation
3. It is useful to have thin ribs/bosses as the lastpoint to fill
25. HESITATION
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 146/158
146
point to fill
4. Increase the wall thickness where the hesitationoccurred, to reduce the resistance to flow.
5. Use a less viscous material
6. Inject more quickly
7. Increase the melt temp
Over packing is when extra material is compressedin one flow path while other flow paths are stillfilling.
26. OVERPACKING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 147/158
147
26. OVERPACKING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 148/158
148
Remedies for Over packing
1. Thicken or thin parts of the model to act as flowleaders or deflectors.
26. OVERPACKING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 149/158
149
2. Move the injection location to a position that willdefine similar length flow paths.
3. Divide the cavity into imaginary sections, anduse one injection location for each section.
4. Remove unnecessary gates.
Unbalanced flow is plastic completely fillingsome flow paths in the mold before other flow
paths have filled.
27. UNBALANCED FLOW
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 150/158
150
27. UN BALANCED FLOW
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 151/158
151
Remedies for Unbalanced flow
1. By altering the thickness of regions within thepart, flow can be fastened or delayed incertain directions to help balance flows.
27. UN BALANCED FLOW
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 152/158
152
p
28. NOZZLE DROOL
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 153/158
153
28. NOZZLE DROOL
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 154/158
154
29. NOZZLE FREEZE - OFF
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 155/158
155
29. NOZZLE FREEZE - OFF
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 156/158
156
30 . NOZZLE SPITTING
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 157/158
157
31. SCREW SLIP
7/27/2019 MOULDING DEFECTS 1.PDF
http://slidepdf.com/reader/full/moulding-defects-1pdf 158/158
158