Submittal:
Welding Procedures/ Welder Qualifications
Electrode Specifications
Orange County Sanitation District P1-P101
Sludge Dewatering & Odor Control at Plant 1
Orange County, California
![Page 2: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/2.jpg)
![Page 3: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/3.jpg)
![Page 4: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/4.jpg)
Page 1 of 2
ASC-982-Shop-FCAW-FP-1
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Shop-FCAW-FP-1WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW Type:
JOINTType Corner, T-joint
Backing Material Weld Metal
Root Opening Root Face Dimension0-1/8" 0-1/8"
Groove Angle Radius (J-U)45 deg N/A
Method Air-Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-1
Hobart
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
Argon/C0275/2540 CFH
.625
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
Excel Arc 71
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No
R
T1
BACKGOUGE
f
α
Single-bevel-groove weld (4)
Corner joint (C)T-joint (T)
T2
NotAl lUUGMAWFCAW required
UTC-U4b-GF
Root OpeningRoot FaceGroove Angle
WeldingProcess
JointDesignation T1 T2
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
G
AD
Base MetalThickness
JK
(see 3.13.1) (see 3.13.1)
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-1 1/16" DCEP 245 amps 25 14
All FCAW E71T-1 .045 DCEP 220 amps 25 8
+ or - + or - + or -
10% 7% 25%
![Page 5: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/5.jpg)
Page 2 of 2
ASC-982-Shop-FCAW-FP-1
Allied Steel Company, IncWelding Procedure Specification
MEMO
R
T1
BACKGOUGE
f
α
Single-bevel-groove weld (4)
Corner joint (C)T-joint (T)
T2
NotAl lUUGMAWFCAW required
UTC-U4b-GF
Root OpeningRoot FaceGroove Angle
WeldingProcess
JointDesignation T1 T2
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
G
AD
Base MetalThickness
JK
(see 3.13.1) (see 3.13.1)
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
![Page 6: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/6.jpg)
Page 1 of 2
ASC-982-Shop-FCAW-FP-2
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Shop-FCAW-FP-2WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW Type:
JOINTType Corner, T-joint
Backing Material Weld Metal
Root Opening Root Face Dimension0-1/8" 0-1/8"
Groove Angle Radius (J-U)45 deg N/A
Method Air-Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-1
Hobart
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
Argon/C0275/2540 CFH
.625
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
Excel Arc 71
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No
R
T1
T2
Corner joint (C)T-joint (T) BACKGOUGE
Al lU
f
α
α
Double-bevel-groove weld (5)
UGMAWFCAW
TC-U5-GFNot
required
Root OpeningRoot FaceGroove Angle
WeldingProcess
JointDesignation T1 T2
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
G
AD
Base MetalThickness
JK
H
(see 3.13.1) (see 3.13.1)
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-1 1/16" DCEP 245 amps 25 14
All FCAW E71T-1 .045 DCEP 220 amps 25 8
+ or - + or - + or -
10% 7% 25%
![Page 7: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/7.jpg)
Page 2 of 2
ASC-982-Shop-FCAW-FP-2
Allied Steel Company, IncWelding Procedure Specification
MEMO
R
T1
T2
Corner joint (C)T-joint (T) BACKGOUGE
Al lU
f
α
α
Double-bevel-groove weld (5)
UGMAWFCAW TC-U5-GF Not
required
Root OpeningRoot FaceGroove Angle
WeldingProcess
JointDesignation T1 T2
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
G
AD
Base MetalThickness
JK
H
(see 3.13.1) (see 3.13.1)
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
![Page 8: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/8.jpg)
Page 1 of 2
ASC-982-Shop-FCAW-FP-3
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Shop-FCAW-FP-3WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW Type:
JOINTType Butt
Backing Material Weld Metal
Root Opening Root Face Dimension0-1/8" 0-1/8"
Groove Angle Radius (J-U)45 deg N/A
Method Air-Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-1
Hobart
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
Argon/C0275/2540 CFH
.625
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
Excel Arc 71
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No
Al lUU -
R
T1
BACKGOUGE
f
α
Butt joint (B)Single-bevel-groove weld (4)
GMAWFCAW
B-U4b-GF Notrequired
Root OpeningRoot Face
Groove AngleWeldingProcess
JointDesignation T1 T2
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
D
AC
Base MetalThickness
J
(see 3.13.1) (see 3.13.1)( U=unlimited )
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8
Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-1 1/16" DCEP 245 amps 25 14
All FCAW E71T-1 .045 DCEP 220 amps 25 8
+ or - + or - + or -
10% 7% 25%
![Page 9: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/9.jpg)
Page 2 of 2
ASC-982-Shop-FCAW-FP-3
Allied Steel Company, IncWelding Procedure Specification
MEMO
Al lUU -
R
T1
BACKGOUGE
f
α
Butt joint (B)Single-bevel-groove weld (4)
GMAWFCAW
B-U4b-GF Notrequired
Root OpeningRoot Face
Groove AngleWeldingProcess
JointDesignation T1 T2
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
D
AC
Base MetalThickness
J
(see 3.13.1) (see 3.13.1)( U=unlimited )
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8
Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
![Page 10: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/10.jpg)
Page 1 of 2
ASC-982-Shop-FCAW-FW-1
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Shop-FCAW-FW-1WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW
Prequalified, Fillet
Type:
JOINTType Corner, Lap, T-joint
Backing Material Base Metal
Root Opening Root Face Dimension0-1/16 N/A
Groove Angle Radius (J-U)N/A N/A
Method
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
NA
Any
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-1
Hobart
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
Argon/C0275/2540 CFH
.625
POSITIONPosition of Groove FilletVertical Progression:
N/A All
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
AWS D1.1, 2010
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
Excel Arc 71
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No° °
°
°°
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-1 1/16" DCEP 245 amps 25 14
All FCAW E71T-1 .045 DCEP 220 amps 25 8
+ or - + or - + or -
10% 7% 25%
![Page 11: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/11.jpg)
Page 2 of 2
ASC-982-Shop-FCAW-FW-1
Allied Steel Company, IncWelding Procedure Specification
MEMO
° °°
°°
![Page 12: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/12.jpg)
Page 1 of 2
ASC-982-Field-FCAW-FP-1
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Field-FCAW-FP-1WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW Type:
JOINTType Corner, T-joint
Backing Material Metal Bar
Root Opening Root Face Dimension1/4" N/A
Groove Angle Radius (J-U)45deg N/A
Method Air Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-8
Lincoln
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
N/AN/AN/A
N/A
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32- 225 F
32- 225 F N/A None N/A
Authorized By Date
Revision
Unlimited
NA-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
NR232
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
NoCorner joint (C)
α
T1
T2
R
Single-bevel-groove-weld (4)T-joint (T)
U R = 3/8 = 30°GMAWFCAW
R = 3/16
R = 1/4
= 30°
= 45°
TC-U4a-GF U
Al l
F
Al l
Notes
GA
WeldingProcess
JointDesignation T1
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
RootOpeningT 2
Base MetalThickness
GrooveAngle
Required
Not req.
Not req.JK
(see 3.13.1) (see 3.13.1)
R = +1/16, -0
= +10°, -0°
+1/4, -1/16
+10°, -5°
α
α
αα
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-8 .072 DCEN 255 amps 23 14
All FCAW E71T-8 .068 DCEN 250 amps 21 8
+ or - + or - + or -
10% 7% 25%
![Page 13: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/13.jpg)
Page 2 of 2
ASC-982-Field-FCAW-FP-1
Allied Steel Company, IncWelding Procedure Specification
MEMO
Corner joint (C)α
T1
T2
R
Single-bevel-groove-weld (4)T-joint (T)
U R = 3/8 = 30°GMAWFCAW
R = 3/16
R = 1/4
= 30°
= 45°
TC-U4a-GF U
Al l
F
Al l
Notes
GA
WeldingProcess
JointDesignation T1
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
RootOpeningT 2
Base MetalThickness
GrooveAngle
Required
Not req.
Not req.JK
(see 3.13.1) (see 3.13.1)
R = +1/16, -0= +10°, -0°
+1/4, -1/16+10°, -5°
α
α
αα
![Page 14: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/14.jpg)
Page 1 of 2
ASC-982-Field-FCAW-FP-2
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Field-FCAW-FP-2WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW Type:
JOINTType Butt
Backing Material Weld Metal
Root Opening Root Face Dimension0-1/8" 0-1/8"
Groove Angle Radius (J-U)45deg N/A
Method Air Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-8
Lincoln
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
N/AN/AN/A
N/A
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32- 225 F
32- 225 F N/A None N/A
Authorized By Date
Revision
Unlimited
NA-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
NR232
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No
Al lUU -
R
T1
BACKGOUGE
f
α
Butt joint (B)Single-bevel-groove weld (4)
GMAWFCAW
B-U4b-GF Notrequired
Root OpeningRoot Face
Groove AngleWeldingProcess
JointDesignation T1 T2
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
D
AC
Base MetalThickness
J
(see 3.13.1) (see 3.13.1)( U=unlimited )
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8
Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-8 .072 DCEN 255 amps 23 14
All FCAW E71T-8 .068 DCEN 250 amps 21 8
+ or - + or - + or -
10% 7% 25%
![Page 15: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/15.jpg)
Page 2 of 2
ASC-982-Field-FCAW-FP-2
Allied Steel Company, IncWelding Procedure Specification
MEMO
Al lUU -
R
T1
BACKGOUGE
f
α
Butt joint (B)Single-bevel-groove weld (4)
GMAWFCAW
B-U4b-GF Notrequired
Root OpeningRoot Face
Groove AngleWeldingProcess
JointDesignation T1 T2
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions
Gas Shieldingfor FCAW
Notes
D
AC
Base MetalThickness
J
(see 3.13.1) (see 3.13.1)( U=unlimited )
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8
Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
![Page 16: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/16.jpg)
Page 1 of 2
ASC-982-Field-FCAW-FW-1
Allied Steel Company, IncWelding Procedure Specification
ASC-982-Field-FCAW-FW-1WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
FCAW
Prequalified, Fillet
Type:
JOINTType Corner, Lap, T-joint
Backing Material Base Metal
Root Opening Root Face Dimension0-1/16 N/A
Groove Angle Radius (J-U)N/A N/A
Method
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
NA
Any
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.20
E71T-8
Lincoln
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
N/AN/AN/A
N/A
POSITIONPosition of Groove FilletVertical Progression:
N/A All
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
3/4-1"
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32- 225 F
32- 225 F N/A None N/A
Authorized By Date
Revision
AWS D1.1, 2010
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
NR232
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No° °
°
°°
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All FCAW E71T-8 .072 DCEN 255 amps 23 14
All FCAW E71T-8 .068 DCEN 250 amps 21 8
+ or - + or - + or -
10% 7% 25%
![Page 17: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/17.jpg)
Page 2 of 2
ASC-982-Field-FCAW-FW-1
Allied Steel Company, IncWelding Procedure Specification
MEMO
° °°
°°
![Page 18: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/18.jpg)
Page 1 of 2
ASC-982-Field-SMAW-FP-1
Allied Steel Company, Inc.Welding Procedure Specification
ASC-982-Field-SMAW-FP-1WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
SMAW Type:
JOINTType Corner, T-joint
Backing Material Metal Bar
Root Opening Root Face Dimension1/4" N/A
Groove Angle Radius (J-U)45 deg N/A
Method Air-Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.1
E7018
Lincoln
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
N/AN/AN/A
N/A
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
N/A
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
7018 MR
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No
WeldingProcess
JointDesignation T1
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions Notes
RootOpeningT 2
Base MetalThickness
GrooveAngle
U= 30°
UR = 3/8
R = 1/4 = 45°SMAW TC-U4a
Al l
F,V,OH E, G, J, K
E, G, J, K
Corner joint (C) α
T1
T2
R
Single-bevel-groove-weld (4)T-joint (T)
(see 3.13.1) (see 3.13.1)
R = +1/16, -0= +10°, -0°
+1/4,-1/16
+10°, -5°α
α
α
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All SMAW E7018 1/8" DCEP 90-160 N/A as req.
All SMAW E7018 5/32" DCEP 130-210 N/A as req.
![Page 19: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/19.jpg)
Page 2 of 2
ASC-982-Field-SMAW-FP-1
Allied Steel Company, Inc.Welding Procedure Specification
MEMO
WeldingProcess
JointDesignation T1
(U=unlimited)
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions Notes
RootOpeningT 2
Base MetalThickness
GrooveAngle
U= 30°
UR = 3/8
R = 1/4 = 45°SMAW TC-U4a
Al l
F,V,OH E, G, J, K
E, G, J, K
Corner joint (C) α
T1
T2
R
Single-bevel-groove-weld (4)T-joint (T)
(see 3.13.1) (see 3.13.1)
R = +1/16, -0= +10°, -0°
+1/4,-1/16+10°, -5°α
α
α
![Page 20: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/20.jpg)
Page 1 of 2
ASC-982-Field-SMAW-FP-2
Allied Steel Company, Inc.Welding Procedure Specification
ASC-982-Field-SMAW-FP-2WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
SMAW Type:
JOINTType Butt
Backing Material Weld Metal
Root Opening Root Face Dimension0-1/8" 0-1/8"
Groove Angle Radius (J-U)45 deg N/A
Method Air-Arc
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
Unlimited
NA
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.1
E7018
Lincoln
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
N/AN/AN/A
N/A
POSITIONPosition of Groove FilletVertical Progression:
All N/A
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
N/A
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
7018 MR
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No
SMAWSMAW Al lU -
Butt joint (B)Single-bevel-groove weld (4)
B-U4b
R
T1
BACKGOUGE
f
α
C, D
WeldingProcess
JointDesignation T1
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions NotesT 2
Base MetalThickness Root Opening
Root FaceGroove Angle
E, J
(see 3.13.1) (see 3.13.1)( U=unlimited )
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All SMAW E7018 1/8" DCEP 90-160 N/A as req.
All SMAW E7018 5/32" DCEP 130-210 N/A as req.
![Page 21: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/21.jpg)
Page 2 of 2
ASC-982-Field-SMAW-FP-2
Allied Steel Company, Inc.Welding Procedure Specification
MEMO
SMAWSMAW Al lU -
Butt joint (B)Single-bevel-groove weld (4)
B-U4b
R
T1
BACKGOUGE
f
α
C, D
WeldingProcess
JointDesignation T1
Groove PreparationTolerances
As Detailed As Fit UpPermitted WeldingPositions NotesT 2
Base MetalThickness Root Opening
Root FaceGroove Angle
E, J
(see 3.13.1) (see 3.13.1)( U=unlimited )
+10° , -0° +10° , -5°= 45°
R = 0 to 1/8Not limited+1/16, -0f = 0 to 1/8
+1/16, -0 +1/16, -1/8
α
![Page 22: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/22.jpg)
Page 1 of 2
ASC-982-Field-SMAW-FW-1
Allied Steel Company, Inc.Welding Procedure Specification
ASC-982-Field-SMAW-FW-1WPS No. Date By3/14/2014 Gary Chapman
Welding Process(es)
Supporting PQR(s)
SMAW Type:
JOINTType Corner, Lap, T-joint
Backing Material Base Metal
Root Opening Root Face Dimension0-1/16 N/A
Groove Angle Radius (J-U)N/A N/A
Method
BASE METALSMaterial Spec.
Type or Grade
Thickness: Groove ( )
Fillet ( )
NA
Any
A36, A572 A992, A500to
50, Grade Bto36, 50
Diameter (Pipe, ) NA
FILLER METALSAWS Specification
AWS Classification
5.1
E7018
Lincoln
SHIELDINGFlux Gas
CompositionFlow Rate
Gas Cup Size
Electrode-Flux (Class)N/A
N/A
N/AN/AN/A
N/A
POSITIONPosition of Groove FilletVertical Progression:
N/A All
ELECTRICAL CHARACTERISTICSTransfer Mode (GMAW):
Current:
OtherTungsten Electrode (GTAW):
Size TypeN/A N/A
TECHNIQUEStringer or Weave Bead
Multi-pass or Single Pass (per side)
Number of Electrodes
Electrode Spacing: LongitudinalLateral
Angle
Contact Tube to Work Distance
Peening
Interpass Cleaning
StringerBoth
1N/AN/AN/A
N/A
NoneDeslag/Wire Brush
PREHEATPreheat Temp., Min.
Interpass Temp., Min. Max.
POSTWELD HEAT TREATMENT
Temp. Time
32 - 225 F
32 - 225 F N/A None N/A
Authorized By Date
Revision
Unlimited-
-
-
Thickness Up to 3/4" Temperature
Over 3/4" to 1-1/2"
Over 1-1/2" to 2-1/2"
Over 2-1/2"
WELDING PROCEDURE
Gary Chapman 3/14/2014
0
50F
150F
32F
225F
7018 MR
Backing
Back Gouge
Manual Machine AutoSemi-Auto
Yes
Yes
Single Weld Double Weld
Up Down
Short-Circuiting Globular Spray
AC DCEP DCEN Pulsed
PWHT Required
Prequalified
No° °
°
°°
No
Layer/Pass Process Filler Metal Class Diameter Cur. Type Amps or WFS Volts Travel Speed Other Notes
All SMAW E7018 1/8" DCEP 90-160 N/A as req.
All SMAW E7018 5/32" DCEP 130-210 N/A as req.
![Page 23: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/23.jpg)
Page 2 of 2
ASC-982-Field-SMAW-FW-1
Allied Steel Company, Inc.Welding Procedure Specification
MEMO
° °°
°°
![Page 24: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/24.jpg)
![Page 25: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/25.jpg)
![Page 26: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/26.jpg)
![Page 27: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/27.jpg)
![Page 28: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/28.jpg)
![Page 29: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/29.jpg)
![Page 30: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/30.jpg)
![Page 31: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/31.jpg)
![Page 32: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/32.jpg)
![Page 33: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/33.jpg)
![Page 34: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/34.jpg)
![Page 35: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/35.jpg)
Certificate of Conformanceto Requirements for Welding Electrode
EXCEL-ARC 71Product Type:
E71T-1C/M,E71T-9C/M; T46 3 PC/M2H10Classification:
A5.20, SFA 5.20; EN17632-ASpecifications:
1/16"Diameter Tested:
06/16/2011Date Tested:
6/16/2011Date Generated:This is to certify that the product named above and supplied on the referenced order number is of the same classification, manufacturing process, and material requirements as the material which was used for the test that was concluded on the date shown, the results of which are shown below. All tests required by the specifications shown for classification were performed at that time and the material tested met all requirements. It was manufactured and supplied by the Quality System Program of Hobart Brothers, which meets the requirements of ISO9000, ANSI/AWS A5.01, and other specification and Military requirements, as applicable.
Test SettingsWFS Travel Speed Shielding Medium Amps / Polarity Volts ESO in(mm) Preheat F(C) Interpass F(C)in/min(m/min) in/min(cm/min)
SG-C 300 / DCEP 26 280 (7.1) 3/4 (19) 60(16) 300(149) 10 (25.4)SG-AC-25 300 / DCEP 26 280 (7.1) 3/4 (19) 60(16) 300(149) 10 (25.4)
Mechanical Properties - TensileShielding Medium Ref. No. Testing Conditions Ult. Tensile Strength psi Yield Strength psi (MPa) Elong.% in 2"
(MPa)SG-C PB3989 Aged 48 Hrs 200F 84,000 ( 582 ) 77,000 ( 531 ) 28
SG-AC-25 PB3992 Aged 48 Hrs 200F 90,000 ( 619 ) 83,000 ( 571 ) 26
Mechanical Properties - ImpactShielding Medium Ref. No. Testing Conditions Temp. F (C) Individuals ft.lb.(J) Avg. ft.lb.(J) Type
SG-C PB3989 As Welded 0 (-18) 102,96,106 (138,130,144) 101 ( 137 ) Charpy-V-NotchSG-C PB3989 As Welded -20 (-29) 78,70,92 (106,95,125) 80 ( 108 ) Charpy-V-Notch
SG-AC-25 PB3992 As Welded 0 (-18) 93,95,84 (126,129,114) 91 ( 123 ) Charpy-V-NotchSG-AC-25 PB3992 As Welded -20 (-29) 72,60,76 (98,81,103) 69 ( 94 ) Charpy-V-Notch
Ref.No. Radiographic Inspection Fillet Weld TestPB3989 Conforms Horizontal : Overhead : Conforms Vertical : ConformsPB3992 Conforms Horizontal : Overhead : Conforms Vertical : Conforms
Chemical AnalysisShielding Medium / Ref. No C Mn P S Si Cu Cr V Ni Mo Al Ti Nb Co B W Sn Fe Sb N Mg Zn Be
SG-C / CB20032 0.02 1.28 0.002 0.004 0.42 0.02 0.04 0.02 0.01 0.01SG-AC-25 / CB20042 0.02 1.50 0.002 0.005 0.54 0.02 0.04 0.02 0.01 0.01
Diffusible Hydrogen Collected per AWS A4.3SG-C 5.2 ml/100g of weld metal for 1/16 in diameter
SG-AC-25 4.8 ml/100g of weld metal for 1/16 in diameter
Joe O'Leary, Quality Assurance Rep.
Certification and Limited Warranty - Data for the above supplied product are those obtained when welded and tested in accordance with the above specification. All tests for the above classification were satisfied. Other tests and procedures may produce different results. Hobart Brothers produces welding consumables under continuing quality assurance programs audited and approved by the American Bureau of Shipping ("ABS").
![Page 36: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/36.jpg)
FEATURES: BENEFITS: • Low fumes and spatter • Increases welder appeal and productivity • Easy slag removal • Reduces clean-up time, minimizes risk of inclusions • Bridges poor fit-up • Increases productivity, reduces part rejection • Good impact strength at low temperatures • Resists cracking in severe applications
APPLICATIONS: • Non-alloyed and fine grain steels • Structural Steel • General Fabrication • Heavy Equipment
SLAG SYSTEM: Fast freezing, rutile type, flux-cored wire
SHIELDING GAS: 100% Carbon Dioxide (CO2), 75% Argon (Ar)/25% Carbon Dioxide (CO2), 35-50 cfh (14-24 l/min)
TYPE OF CURRENT: Direct Current Electrode Positive (DCEP)
STANDARD DIAMETERS: 0.035” (0.9 mm), 0.045” (1.2 mm), 0.052” (1.4 mm), 1/16” (1.6 mm)
RE-DRYING: Not recommended
STORAGE: Product should be stored in a dry, enclosed environment, and in its original intact packaging
TYPICAL WELD METAL CHEMISTRY* (Chem Pad):
Note: AWS specification single values are maximums.
TYPICAL DIFFUSIBLE HYDROGEN*:
TYPICAL MECHANICAL PROPERTIES* [Aged 48 hrs @ 200°F (93°C)]:
TYPICAL CHARPY V-NOTCH IMPACT VALUES* (AS WELDED):
*The information contained or otherwise referenced herein is presented only as “typical” without guarantee or warranty, and Hobart Brothers Company expressly disclaims any liability incurred from any reliance thereon. Typical data are those obtained when welded and tested in accordance with AWS A5.20 specification. Other tests and procedures may produce different results. No data is to be construed as a recommendation for any welding condi-tion or technique not controlled by Hobart Brothers Company.
Weld Metal Analysis 100% CO2 75% Ar/25% CO2
Carbon (C) 0.021 0.022 Manganese (Mn) 1.30 1.60 Silicon (Si) 0.69 0.82 Sulphur (S) 0.011 0.010
Phosphorus (P) 0.015 0.014
AWS Spec
0.12 1.75 0.90 0.03
0.03
5.2ml/100g 4.8100g
(GAS CHROMATOGRAPHY)
Hydrogen Equipment 100% CO2 75% Ar/25% CO2 AWS Spec
8.0ml/100g Maximum
Tensile Strength 84,000 psi (582 MPa) 90,000 psi (619 MPa) Yield Strength 77,000 psi (531 MPa) 83,000 psi (571 MPa) Elongation % in 2” (50 mm) 28% 26%
70,000-95,000 psi (490-670 MPa) 58,000 psi (390 MPa) Minimum
22% Minimum
Mechanical Tests 100% CO2 75% Ar/25% CO2 AWS Spec
Avg. at 0°F (-20°C) 101 ft•lbs (137 Joules) 91 ft•lbs (123 Joules)
Avg. at -20°F (-30°C) 80 ft•lbs (108 Joules) 69 ft•lbs (94 Joules)
20 ft•lbs (27 Joules) Minimum
20 ft•lbs (27 Joules) Minimum
CVN Temperatures 100% CO2 75% Ar/25% CO2 AWS Spec
Excel Arc 71
AWS A5.20: E71T-1C H8, E71T-1M H8, E71T-9C H8, E71T-9M H8 EN17632-A: T 46 3 P C/M 2 H10
Hobart Brothers Company 101 Trade Square East Troy, OH 45373 PH: (800) 424-1543 FX: 800-541-6607 www.hobartbrothers.com
WELDING POSITIONS:
![Page 37: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/37.jpg)
Excel Arc 71
Diameter
Inches (mm)
Weld
Position
Amps
Volts
Wire-Feed Speed
in/min (m/min)
Deposition Rate
lbs/hr (kg/hr)
Contact Tip to Work Distance
Inches (mm)
0.035 (0.9) 0.035 (0.9) 0.035 (0.9) 0.035 (0.9) 0.035 (0.9)
All Position All Position All Position
Flat & Horizontal Flat & Horizontal
125 150 175 200 225
23 24 25 26 28
330 (8.4) 410 (10.4) 545 (13.5) 645 (16.4) 785 (19.9)
3.8 (1.7) 4.7 (2.1) 6.3 (2.9) 7.6 (3.4) 9.4 (4.3)
1/2 (13) 1/2 (13) 1/2 (13) 1/2 (13) 1/2 (13)
0.045 (1.2) 0.045 (1.2) 0.045 (1.2) 0.045 (1.2) 0.045 (1.2) 0.045 (1.2)
All Position All Position All Position All Position
Flat & Horizontal Flat & Horizontal
170 185 200 220 260 300
23 24 25 25 27 29
260 (6.6) 310 (7.9) 302 (7.7) 383 (9.7) 500 (12.7) 590 (15.0)
4.4 (2.0) 6.1 (2.7) 6.2 (2.8) 7.5 (3.4) 8.9 (4.0) 12.3 (5.6)
5/8 (16) 5/8 (16) 5/8 (16) 3/4 (19) 3/4 (19) 3/4 (19)
0.052 (1.4) 0.052 (1.4) 0.052 (1.4)0.052 (1.4) 0.052 (1.4) 0.052 (1.4)
All Position All Position All Position
Flat & Horizontal Flat & Horizontal Flat & Horizontal
170 200 250 260 300 350
24 25 26 27 28 30
191 (4.8) 210 (5.3) 275 (7.0) 320 (8.1) 381 (9.6) 571 (14.5)
5.0 (2.3) 5.6 (2.5) 7.5 (3.4) 8.1 (3.7) 9.5 (4.3) 14.4 (6.5)
3/4 (19) 3/4 (19) 3/4 (19) 3/4 (19) 1 (25) 1 (25)
1/16 (1.6) 1/16 (1.6) 1/16 (1.6) 1/16 (1.6) 1/16 (1.6) 1/16 (1.6)
All Position All Position All Position
Flat & Horizontal Flat & Horizontal Flat & Horizontal
215 245 275 280 360 400
24 25 26 27 28 30
160 (4.1) 189 (4.8) 225 (5.7) 237 (6.0) 328 (8.4) 430 (10.9)
5.6 (2.5) 6.5 (3.0) 7.8 (3.5) 9.3 (4.2) 12.0 (5.4) 16.5 (7.5)
1 (25) 1 (25) 1 (25) 1 (25) 1 (25) 1 (25)
STANDARD DIAMETERS AND PACKAGES: For a complete list of diameters and packaging, please contact Hobart Brothers at (800) 424-1543, or (937) 332-5188 for International Customer Service.
• Maintaining a proper welding procedure - including pre-heat and interpass temperatures - may be critical depending on the type and thickness of steel being welded. • See Above: This information was determined by welding with 100% CO2 shielding gas with a flow rate between 35-50 cfh (14-24 l/min). For 75% Ar/25% CO2 shielding gas, reduce voltage by 1 volt. • All positions include: Flat, Horizontal, Vertical Up, and Overhead.
Diameter
Inches (mm) 33-lb. (15kg)
Spool 44-lb. (20kg)
Spool 60-lb. (27kg)
Coil
0.035 (0.9) S247108-029 — —
0.045 (1.2) S247112-029 S247112-044 —
0.052 (1.4) S247115-029 S247115-044 —
1/16 (1.6) S247119-029 S247119-044 S247119-002
CONFORMANCES AND APPROVALS: • AWS A5.20, E71T-1C H8, E71T-1M H8, E71T-9C H8, E71T-9M H8 • AWS A5.20M, E491T-1C H8, E491T-1M H8, E491T-9C H8, E491T-9M H8 • ASME SFA 5.20, E71T-1C H8, E71T-1M H8, E71T-9C H8, E71T-9M H8 • ABS, 100% CO2 3YSA H10, 75% Ar/25% CO2 , 3YSA H10 • Burea Veritas, S3YM HH • CWB, 100% CO2 E491T-9-H8, 75-80% Ar/Balance CO2, E491T-9M-H8 • DNV, III Y40MS (H10) • EN17632-A: T 46 3 P C/M 2 H10 • Lloyd’s Register, 100% CO2 3YS H10 • AWS D1.8 Conformance: 1/16” (1.6 mm) diameter electrode with 100% CO2 or 75% Ar/25% CO2 shielding gases
CAUTION: Consumers should be thoroughly familiar with the safety precautions on the warning label posted in each shipment and in the American National Standard Z49.1, “Safety in Welding and Cutting,” published by the American Welding Society, 550 NW LeJune Road, Miami, FL 33126; OSHA Safety and Health Standards 29 CFR 1910 is available from the U.S. Department of Labor, Washington, D.C. 20210 Material Safety Data Sheets on any Hobart Brothers Company product may be obtained from Hobart Customer Service or at www.hobartbrothers.com.
Because Hobart Brothers Company is constantly improving products, Hobart reserves the right to change design and/or specifications without notice.
Excel Arc is a trademark of Hobart Brothers Company, Troy, Ohio.
Revision Date: 110613 (Replaces 100708) 636-Y, INDEX
![Page 38: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/38.jpg)
The Lincoln Electric Company
22801 St. Clair Avenue
Cleveland, Ohio 44117-1199
CERTIFICATE OF CONFORMANCE(APPLIES ONLY TO U.S. PRODUCTS)
Excalibur® 7018 MRProduct: [1Year]
E7018H4RClassification:
Specification: AWS A5.1:2004, ASME SFA-5.1
January 04, 2012Date
This is to certify that the product named above and supplied on the referenced order number is of the same classification, manufacturing process, and material requirements as the material
which was used for the test that was concluded on the date shown, the results of which are shown below. All tests required by the specifications shown for classification were performed at
that time and the material tested met all requirements. It was manufactured and supplied according to the Quality System Program of the Lincoln Electric Company, Cleveland, Ohio, U.S.A.,
which meets the requirements of ISO9001, NCA3800, AWS A5.01, and other specification and Military requirements, as applicable. The Quality System Program has been approved by
ASME, ABS, and VdTUV.
AWS/ASMERequirements RESULTS
294 1 2 3 4Electrode Size 5/32 inch 5/32 inch 3/16 inch 3/16 inchPolarity AC DC+ AC DC+Plate Thickness, mm (in) 19 (3/4) 19 (3/4) 19 (3/4) 19 (3/4)Current, A 180 170 240 210Pass/Layers 14/7 14/7 14/7 14/7Preheat Temperature, °C (°F) (225 min.) 120 (250) 120 (250) 120 (250) 120 (250)Interpass Temperature, °C (°F) (225 - 350) 165 (325) 165 (325) 165 (325) 165 (325)Postweld Heat Treatment As-welded As-welded As-welded As-welded As-welded
Operating Settings
Mechanical properties of weld deposits
Tensile Strength, MPa (ksi) (70 min.) 520 (75) 510 (74) 550 (79) 540 (78)Yield Strength, 0.2% Offset, MPa (ksi) (58 min.) 430 (62) 420 (60) 450 (65) 450 (65)
Elongation 22 min. 36 33 33 30
Average Impact Energy (20 min.) 314 (232) 336 (248) 162 (119) 139 (102)Joules @ -29 °C (ft-lbs @ -20 °F) 211,350,381 (156,258,281) 216,395,399 (159,291,294) 144,156,186 (106,115,137) 98,153,165 (72,113,122)
Average Hardness, HRB Not Required 84 84 86 86
Chemical composition of weld deposits (weight %)
C 0.15 max. 0.05 0.04 0.05 0.05Mn 1.60 max. 1.08 1.12 1.12 1.09Si 0.75 max. 0.42 0.41 0.51 0.49S 0.035 max. 0.006 0.005 0.005 0.005P 0.035 max. 0.014 0.014 0.013 0.013Cr 0.20 max. 0.03 0.04 0.03 0.03Ni 0.30 max. 0.05 0.05 0.03 0.03Mo 0.30 max. 0.01 0.01 0.01 0.01V 0.08 max. 0.01 0.01 0.01 0.01
Mn+Ni+Cr+Mo+V 1.75 max. 1.18 1.23 1.21 1.17
Requirements RESULTS294 1 2 3 4
Electrode Size 3/32 inch 3/32 inch 1/4 inch 1/4 inchPolarity AC DC+ AC DC+Diffusible Hydrogen, mL/100g 4 max. 2 3 3 3Absolute Humidity (grains moisture/lb dry air) 55 55 65 65
Diffusible Hydrogen (per AWS A4.3)
Requirements RESULTS
294 1 2 3Electrode Size 3/32 inch 5/32 inch 1/4 inchCoating moisture - As received 0.3 max. 0.1 0.1 0.1Coating moisture - Humidified 0.4 max. 0.3 Not Required 0.4
Moisture
Page 1 of 2 Cert. No. 31758
![Page 39: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/39.jpg)
The Lincoln Electric Company
22801 St. Clair Avenue
Cleveland, Ohio 44117-1199
CERTIFICATE OF CONFORMANCE(APPLIES ONLY TO U.S. PRODUCTS)
Excalibur® 7018 MRProduct: [1Year]
E7018H4RClassification:
Specification: AWS A5.1:2004, ASME SFA-5.1
January 04, 2012Date
1. This certificate complies with the requirements of EN 10204, Type 2.2
2. The electrode sizes required to be tested for this classification are 5/32 inch, 3/16 inch and 1/4 inch. The 3/32 inch, 1/8 inch and
7/32 inch sizes will also meet these requirements.
3. The 1/4 diameter electrode was reconditioned prior to moisture testing at 800 °F for 1 hour.
4. The 1/4 diameter electrode was reconditioned prior to diffusible testing at 800 °F for 1 hour.
5. Test assembly constructed of ASTM A36 steel.
6. Fillet Weld Test (positions as required): Met requirements.
7. Radiographic Inspection: Grade 1 - Met requirements.
8. Results below the detection limits of the instrument or lower than the precision required by the specification are reported as zero.
Strength values in SI units are reported to the nearest 10 MPa converted from actual data. Preheat and interpass temperature
values in SI units are reported to the nearest 5 degrees.
Toronto Cunningham, Certification Supervisor Date
Dave Fink, Manager, Compliance
Engineering, Consumable R&D
Date
January 04, 2012
January 05, 2012
Page 2 of 2 Cert. No. 31758
![Page 40: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/40.jpg)
26 ı T H E L I N C O L N E L E C T R I C C O M P A N Y
STICK (SMAW) ELECTRODE
Excalibur ® 7018 MR ®
Welding Positions
Typical Applications
All, except vertical down
Mild steel
Power generation
Petrochemical
Pressure vessels
Pressure piping
Premium arc performance
Square coating burn-off
Easy strike and re-strike
Effortless slag removal
Minimal spatter for enhanced operability and clean weld surface
Conformances
Mild Steel, Low Hydrogen • AWS E7018 H4R
Key FeaturesAWS A5.1/A5.1M: 2004ASME SFA-A5.1:ABS:Lloyd’s Register:DNV Grade:GL:BV Grade:CWB/CSA W48-06:EN ISO 2560-B:
E7018 H4RE7018 H4R3Y H53YM H53 YH53YH53YHHHE4918E4918 A H5
DIAMETERS / PACKAGINGDiameter Length 1 lb (0.5 kg) Plastic Tube
6 lb (2.7 kg) Master Carton10 lb (4.5 kg) Easy Open Can30 lb (13.6 kg) Master Carton
50 lb (22.7kg)Cartonin (mm) in (mm)
3/321/8
5/323/167/321/4
(2.4)(3.2)(4.0)(4.8)(5.6)(6.4)
14 (350)14 (350)14 (350)14 (350)18 (450)18 (450)
ED032086ED031468
ED032588ED032589ED032590
ED028280ED028281ED028282ED028283ED028917ED028918
TYPICAL OPERATING PROCEDURESCurrent (Amps)
Polarity(4) 3/32 in (2.4 mm) 1/8 in (3.2 mm) 5/32 in (4.0 mm) 3/16 in (4.8 mm) 7/32 in (5.6 mm) 1/4 in (6.4 mm)
DC+ 70-110 90-160 130-210 180-300 250-330 300-400
AC 80-120 100-160 140-210 200-300 270-370 325-420
MECHANICAL PROPERTIES(1) – As Required per AWS A5.1/A5.1M: 2004
Yield Strength(2) Tensile Strength ElongationCharpy V-Notch
J (ft•lbf)MPa (ksi) MPa (ksi) % @ -29°C (-20°F)
Requirements - AWS E7018 H4R 400 (58) min. 490 (70) min. 22 min. 27 (20) min.
Typical Results(3) - As-Welded 430-510 (62-74) 510-605 (74-88) 25-37 121-332 (89-246)
DEPOSIT COMPOSITION(1) – As Required per AWS A5.1/A5.1M: 2004%C %Mn %Si %P %S %Ni
Requirements - AWS E7018 H4R 0.15 max. 1.60 max. 0.75 max. 0.035 max. 0.035 max. 0.30 max.
Typical Results(3) 0.03-0.08 1.01-1.55 0.34-0.68 0.01-0.02 0.01 0.01-0.06
%Cr %Mo %V%Mn + Ni + Cr
+ Mo + VDiffusible Hydrogen
(mL/100g weld metal)
Requirements - AWS E7018 H4R 0.20 max. 0.30 max. 0.08 max. 1.75 max. 4.0 max.
Typical Results(3) 0.02-0.07 0.05 0.02 1.04-1.75 2-3
(1)Typical all weld metal. (2)Measured with 0.2% offset. (3)See test results disclaimer below. (4)Preferred polarity is listed first.
![Page 41: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/41.jpg)
THE LINCOLN ELECTRIC COMPANY22801 St. Clair Avenue • Cleveland, OH • 44117-1199 • U.S.A.
Phone: +1.216.481.8100 • www.lincolnelectric.com© Lincoln Global, Inc. All Rights Reserved.Issue Date 01/12
CUSTOMER ASSISTANCE POLICY
The Lincoln Electric Company is manufacturing and selling high quality welding equipment, consumables, and cutting equipment. Our challenge is to meet the needs of our customers and to exceed their expectations. On occasion, purchasers may ask Lincoln Electric for information or advice about their use of our products. Our employees respond to inquiries to the best of their ability based on information provided to them by the customers and the knowledge they may have concerning the application. Our employees, however, are not in a position to verify the information provided or to evaluate the engineering requirements for the particular weldment. Accordingly, Lincoln Electric does not warrant or guarantee or assume any liability with respect to such information or advice. Moreover, the provision of such information or advice does not create, expand, or alter any warranty on our products. Any express or implied warranty that might arise from the information or advice, including any implied warranty of merchantability or any warranty of fitness for any customers’ particular purpose is specifically disclaimed.
Lincoln Electric is a responsive manufacturer, but the selection and use of specific products sold by Lincoln Electric is solely within the control of, and remains the sole responsibility of the customer. Many variables beyond the control of Lincoln Electric affect the results obtained in applying these types of fabrication methods and service requirements.
Subject to Change – This information is accurate to the best of our knowledge at the time of printing. Please refer to www.lincolnelectric.com for any updated information.
TEST RESULTS
Test results for mechanical properties, deposit or electrode composition and diffusible hydrogen levels were obtained from a weld produced and tested according to
prescribed standards, and should not be assumed to be the expected results in a particular application or weldment. Actual results will vary depending on many factors,
including, but not limited to, weld procedure, plate chemistry and temperature, weldment design and fabrication methods. Users are cautioned to confirm by qualification
testing, or other appropriate means, the suitability of any welding consumable and procedure before use in the intended application.
Material Safety Data Sheets (MSDS) and Certificates of Conformance are available on our website at www.lincolnelectric.com
![Page 42: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/42.jpg)
The Lincoln Electric Company
22801 St. Clair Avenue
Cleveland, Ohio 44117-1199
CERTIFICATE OF CONFORMANCE(APPLIES ONLY TO U.S. PRODUCTS)
Innershield®NR-232Product: [1Year]
E71T-8-H16Classification:
Specification: AWS A5.20:2005, ASME SFA-5.20
April 25, 2011Date
This is to certify that the product named above and supplied on the referenced order number is of the same classification, manufacturing process, and material
requirements as the material which was used for the test that was concluded on the date shown, the results of which are shown below. All tests required by the
specifications shown for classification were performed at that time and the material tested met all requirements. It was manufactured and supplied according to
the Quality System Program of the Lincoln Electric Company, Cleveland, Ohio, U.S.A., which meets the requirements of ISO9001, NCA3800, AWS A5.01, and
other specification and Military requirements, as applicable. The Quality System Program has been approved by ASME, ABS, and VdTUV.
E71T-8-H16Requirements RESULTS
76 1 2Electrode Size 0.068 inch 5/64 inchPolarity DC- DC-Voltage, V 21 20Wire Feed Speed, cm/min (in/min) 483 (190) 457 (180)Current, A 270 330Average Heat Input, kJ/mm (kJ/in) (35 - 65) 1.4 (36) 1.6 (41)Contact Tip to Work Distance, mm (in) 25 (1) 25 (1)Pass/Layers 15/6 13/6Preheat Temperature, °C (°F) (60 min.) 20 (72) 20 (71)Interpass Temperature, °C (°F) (275 - 325) 165 (325) 165 (325)Postweld Heat Treatment As-welded As-welded As-welded
Operating Settings
Mechanical properties of weld deposits
Tensile Strength, MPa (ksi) (70 - 95) 600 (87) 590 (85)
Yield Strength, 0.2% Offset, MPa (ksi) (58 min.) 470 (69) 470 (69)
Elongation 22 min. 28 29
Average Impact Energy (20 min.) 75 (56) 80 (59)
Joules @ -29 °C (ft-lbs @ -20 °F) 73,76,77 (54,56,57) 80,80,80 (59,59,59)
Average Hardness, HRB Not Required 88 89
Chemical composition of weld deposits (weight %)
C 0.30 max. 0.17 0.16Mn 1.75 max. 0.70 0.63Si 0.60 max. 0.30 0.27S 0.03 max. 0.00 0.01P 0.03 max. 0.01 0.01Cr 0.20 max. 0.03 0.02Ni 0.50 max. 0.02 0.01Mo 0.30 max. 0.01 0.01V 0.08 max. 0.00 0.00
Cu 0.35 max. 0.02 0.02Al 1.8 max. 0.6 0.6
E71T-8-H16Requirements RESULTS
76 1 2Electrode Size 0.068 inch 5/64 inch
Polarity DC- DC-
Diffusible Hydrogen, mL/100g 16.0 max. 6.6 7.9
Absolute Humidity (grains moisture/lb dry air) 29 29
Diffusible Hydrogen (per AWS A4.3)
1. This certificate complies with the requirements of EN 10204, Type 2.2.
2. The electrode sizes required to be tested for this classification are 0.068 inch and 5/64 inch. The 0.072 inch size will also meet these requirements.
3. Test assembly constructed of ASTM A36 steel.
4. Fillet Weld Test (positions as required): Met requirements.
5. Radiographic Inspection: Met requirements.
6. The strength and elongation properties reported here were obtained from tensile specimens artificially aged at 105°C (220°F) for 48 hours.
7. Results below the detection limits of the instrument or lower than the precision required by the specification are reported as zero. Strength values in SI
units are reported to the nearest 10 MPa converted from actual data. Preheat and interpass temperature values in SI units are reported to the nearest
5 degrees.
April 26, 2011
Rich Bollas, Certification Supervisor Date Dave Fink, Manager, Compliance
Engineering, Consumable R&D
April 25, 2011
Date
Page 1 of 1 Cert. No. 22320
![Page 43: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/43.jpg)
[168] T H E L I N C O L N E L E C T R I C C O M P A N Y
FL
UX
-CO
RE
DS
UB
ME
RG
ED
AR
CS
TA
INL
ES
S &
NIC
KE
LH
AR
DF
AC
ING
Innershield ® NR-232FLUX-CORED SELF-SHIELDED (FCAW-S) WIRE
Welding Positions
Typical Applications
All
�Structural fabrication, including those subject to seismic requirements
�General plate fabrication
�Hull plate and stiffener welding on ships and barges
�Machinery parts, tanks, hoppers, racks and scaffolding
�High deposition rates for out-of-position welding
�Penetrating arc
�Fast freezing, easy to remove slag system
�Meets AWS D.18 seismic lot waiver requirements
Conformances
Mild Steel, All PositionAWS E71T-8
Key Features
E71T-8-H16E71T-8-H163YSA3YS H15III YMS H153YH10SSA3YMHE491T-8 H16EN 758 T42 3 Y N 2EN 758 T42 3 Y N 2MIL-71T-8AS
AWS A5.20/A5.20M: 2005ASME SFA-A5.20:ABS: Lloyd’s Register: DNV Grade:GL:BV Grade:CWB/CSA W48-06: DB: TUV:MIL-E-24403/1:*FEMA 353AWS D1.8
DIAMETERS / PACKAGING
Diameter 13.5 lb (6.1 kg) Coil54 lb (24.5 kg) Carton
13.5 lb (6.1 kg) Coil54 lb (24.5 kg)
Hermetically Sealed Pail25 lb (11.3 kg)
Steel Spool
25 lb (11.3 kg)Plastic Spool (Vacuum
Sealed Foil Bag)50 lb (22.6 kg)
Coilin (mm)
0.0680.0725/64
(1.7)(1.8)(2.0)
ED012518ED012522ED012525
ED030232ED030643ED030644ED030647
ED030949ED012519ED012523ED012526
*Military Grade Classification of MIL-71T-8AS for 0.068 in (1.7 mm) and 0.072 in (1.8 mm) diameters only.
Note��FEMA 353 and AWS D1.8 structural steel seismic supplement test data can be found on this product at www.lincolnelectric.com.
Structural Welding Code Seismic Supplement
![Page 44: Submittal: Welding Procedures/ Welder Qualifications](https://reader034.vdocuments.net/reader034/viewer/2022042702/6265047fb07360600e62c053/html5/thumbnails/44.jpg)
[169]W E L D I N G C O N S U M A B L E S C A T A L O G
FL
UX
-CO
RE
DS
UB
ME
RG
ED
AR
CS
TA
INL
ES
S &
NIC
KE
LH
AR
DF
AC
ING
Innershield ® NR-232FLUX-CORED SELF-SHIELDED (FCAW-S) WIRE
(AWS E71T-8)
DEPOSIT COMPOSITION(1) – As Required per AWS A5.20/A5.20M: 2005
%C %Mn %Si %S %P %Al
RequirementsAWS E71T-8 0.30 max. 1.75 max. 0.60 max. 0.03 max. 0.03 max. 1.8 max.
Typical Performance(3) 0.16 - 0.18 0.61 - 0.72 0.26 - 0.33 ≤0.01 ≤0.01 0.5 - 0.8
MECHANICAL PROPERTIES(1) – As Required per AWS A5.20/A5.20M: 2005
Yield Strength(2) Tensile Strength Elongation HardnessCharpy V-Notch
MPa (ksi) MPa (ksi) % Rockwell B @ -29°C (-20°F)
RequirementsAWS E71T-8 400 (58) min. 480 - 655 (70 - 95) 22 min. – 27 (20) min.
Typical Performance(3)
As-Welded 460 - 520 (66 - 75) 575 - 615 (83 - 89) 25 - 31 87 - 90 47 - 75 (35 - 55)
(1)Typical all weld metal. (2)Measured with 0.2% offset. (3)See test results disclaimer on pg. 9.
TYPICAL OPERATING PROCEDURES
Diameter, Polarity
CTWD(6)
mm (in)Wire Feed Speed Voltage(7)
(volts)
Approx. Current(amps)
Melt-Off Rate Deposition Rate Efficiency(%)m/min (in/min) kg/hr (lb/hr) kg/hr (lb/hr)
0.068 in (1.7 mm)DC-
19-32 (3/4-1 1/4)
2.83.33.84.35.06.47.4
(110)(130)(150)(170)(195)(250)(320)
18-1919-2119-2120-2223-2423-2425-27
195225250270300350400
2.32.83.23.54.35.46.9
(5.0)(6.2)(7.1)(7.8)(9.4)(11.8)(15.2)
1.82.02.42.83.24.05.2
(3.9)(4.6)(5.3)(6.1)(7.0)(9.0)(11.4)
78747578747675
0.072 in (1.8 mm)DC-
19-32 (3/4-1 1/4)
2.03.53.94.36.47.4
(80)(140)(155)(170)(250)(290)
16-1818-2119-2220-2322-2423-25
130225240255315350
1.83.13.33.65.36.2
(4.0)(6.8)(7.2)(8.0)(11.7)(13.6)
1.52.52.72.94.35.0
(3.3)(5.5)(6.0)(6.5)(9.6)(11.0)
838183818281
5/64 in (2.0 mm)DC-
19-32 (3/4-1 1/4)
1.52.93.03.34.6
(60)(115)(120)(130)(180)
16-1719-2019-2020-2122-23
145260270285365
1.73.23.33.55.0
(3.7)(7.0)(7.3)(7.8)(10.9)
1.22.52.62.83.9
(2.7)(5.5)(5.7)(6.2)(8.7)
7378787980