wed feb 21-fri feb 23

15
Ambient Pressure Laser Heating and Melting of Pt Foil—Validating BL 12.2.2 Temperature Measurements Wed Feb 21-Fri Feb 23 Pt foil (4 m thin) cut in thin strip and mounted in “Wire melting chamber”. Chamber flooded with Ar gas. Laser Power setting at 25 Amps. Waveplate value upon melting 1.90- 2.04 Volts. This means the laser power at the sample was approx.5 Watts (combined upstream and downstream) Melt determination made by visual observation of “melt pool” and/or flicker of sample. Neutral density filters greatly aid in visual observations. Simultaneous diffraction aided in melt determination, but diffraction signal from sample after heating is very weak due to texturing. Detailed discussion of diffraction signal given below.

Upload: zahi

Post on 13-Jan-2016

41 views

Category:

Documents


0 download

DESCRIPTION

Ambient Pressure Laser Heating and Melting of Pt Foil—Validating BL 12.2.2 Temperature Measurements. Wed Feb 21-Fri Feb 23 Pt foil (4 m m thin) cut in thin strip and mounted in “Wire melting chamber”. Chamber flooded with Ar gas. - PowerPoint PPT Presentation

TRANSCRIPT

Page 1: Wed Feb 21-Fri Feb 23

Ambient Pressure Laser Heating and Melting of Pt Foil—Validating BL 12.2.2 Temperature Measurements

• Wed Feb 21-Fri Feb 23• Pt foil (4 m thin) cut in thin strip and mounted in “Wire melting chamber”. Chamber

flooded with Ar gas.• Laser Power setting at 25 Amps. Waveplate value upon melting 1.90-2.04 Volts. This

means the laser power at the sample was approx.5 Watts (combined upstream and downstream)

• Melt determination made by visual observation of “melt pool” and/or flicker of sample. Neutral density filters greatly aid in visual observations.

• Simultaneous diffraction aided in melt determination, but diffraction signal from sample after heating is very weak due to texturing. Detailed discussion of diffraction signal given below.

Page 2: Wed Feb 21-Fri Feb 23

Pre&Post Heat Pt Foil

~25m

Post-heating observations support melting with appearance of holes in foil, and foil having a different (glassy?) texture.

PreHeating PostHeating

Page 3: Wed Feb 21-Fri Feb 23

Ambient Pressure Laser Heating and Melting of Pt Foil

• Temperature calculation is done by fitting data (corrected for system response) to the Planck function in a wavelength range of 600-800 nm. No wavelength dependent emissivity was applied to the data.

• The melting temperature is calculated as the average of the last temperature when a “solid” observation is made and the first determination when a “melt” observation is made.

• For 3 separate runs with observations made both upstream and downstream, the average melt temperature is determined as 2052+/-29 K. This is close to the literature value of 2041 K.

Page 4: Wed Feb 21-Fri Feb 23

Pt Foil Ambient P Laser Melting:Raw Data

Page 5: Wed Feb 21-Fri Feb 23

Temperature Profile during melt observation of ambient pressure Pt foil

Page 6: Wed Feb 21-Fri Feb 23

Temperature Vs Laser Power• Temperature vs total power at sample

position (upstream + downstream)

• Plot levels off at Pt Tm

• Another supporting piece of evidence for melt indication

Page 7: Wed Feb 21-Fri Feb 23

Diffraction signal from Pt foil at ambient condition right after mounting foil before any heating

20 keVDist: 316.974 mm

X-ray diffraction during laser heating of Pt foil

Page 8: Wed Feb 21-Fri Feb 23

Diffraction signal almost completely disappears on a mm-area after heating to moderate temperatures (barely coupling).

1 single diffraction spot left.

Page 9: Wed Feb 21-Fri Feb 23

Zoom in on diffraction spot

Page 10: Wed Feb 21-Fri Feb 23

Most intense D-value corresponds to (111) of Pt. ~ 2.27 Å

(unsure of why spot is split into 3 peaks) residual strain?

Page 11: Wed Feb 21-Fri Feb 23

In vicinity of melting. Spot broadens and loses intensity

Page 12: Wed Feb 21-Fri Feb 23

During HeatingRoom Temperature

Page 13: Wed Feb 21-Fri Feb 23

Integrated Pt Spot During Heating

T =~2000K~1e-5d/d ~ 2e-5d ~ 2.25 => d + d = 2.295

Spot broadens and shifts to higher dsp.Confirms the alignment of x-ray and laser(diffraction from laser heated spot)

Page 14: Wed Feb 21-Fri Feb 23

Peak sharpens up upon quenching.

Page 15: Wed Feb 21-Fri Feb 23

After melting most intensity recovered to the lowest of the 3 peaks