DCT 100 HS Suction Press Roll 2522

Bearing Inspection Report

Sofidel America

Haines City, FL

Thursday - February 11, 2016

End User

Sofidel America

Contact

Mike Brook, Miguel Ventura

Address

1006 Marley Drive

City, State, Zip

Haines City, FL, 33844

Phone

(863) 547-1100

E-mail

[email protected]; Miguel.ve…

SKF TM/ IS

Lewis Richardson / Wayne Millard

Equipment

DCT 100 HS

Distributor

Miller Bearings Inc.

Contact

Doug Keesling

Address

2505 Drane Field Road

City, State, Zip

Lakeland, FL, 33811

Phone

(863) 701-9500

E-mail

[email protected]

Application

Suction Press Roll

Vendor

Valmet

Contact

David Shuford

Address

25 Beloit Street

City, State, Zip

Aiken, SC, 29805

Phone

803-293-2140

E-mail

[email protected]; …

Vendor Job #

407884

Serial#

2522

Inspection Date: 2016-02-11 Travel Time: 9 hours Inspection Time: 1.5 hours

Wayne S. Millard Pulp and Paper Specialist- SKFSavannah, GA 31410 / tel: (404) 771-3658

http://www.SKF.com

[email protected]

Inspected by Bobby Dwayne Scott

Bearing Inspection Report

As always, we appreciate the opportunity to be of service. Please contact me if you have any questionsand/or/comments.Kind Regards,

This report is confidential and proprietary to SKF and may not bedisclosed to any third party without the express written consent ofSKF. Use of this report is limited to the sole purpose for which itwas provided.

Outer Ring Outside Diameter (OD)Normal5.3.3.2 - Fretting corrosion -@ Minor

Outer Ring Raceway (ORR)5.3.3.3 - False brinelling - Minor5.2.2 - Abrasive wear - Minor5.5.3 - Indentation from debris - Minor

Inner Ring Raceway (IRR)5.2.2 - Abrasive wear - Minor5.5.3 - Indentation from debris - Minor

Lubrication: oil

Inner Ring Bore5.3.3.2 - Fretting corrosion - Minor

Rolling Elements5.3.3.3 - False brinelling - Minor5.2.2 - Abrasive wear - Minor5.5.3 - Indentation from debris - Minor

CageNormal

Tending Bearing Inspection

Sofidel America DCT 100 HS 2522 Suction Press Roll

Recommendations: Reuse Bearing Remanufacture Bearing Replace Bearing

Bearing can be reused and (should/will) be thoroughly cleaned, coated with anti-corrosive material,and protected during storage prior to re-installation on journal bearing seat, per SKF.

Bearing Nomenclature: Inner Race Rotation Outer Race Rotation

SKF 239/630 CAK/C083W33 "E" 2008 REMAN: RG#-6741-R1-P "H" R.L.-.028 "H" 2011

Comments:

Lightly hand scotchbright false brinelling marks, fully clean, and reuse with current ORR load zonerelocated. Also review housing & bearing cleanliness during overhauling, housing sealing design, oilfiltration, roll storage, and roll transit techniques. Contact SKF for further assistance.

Inspection Findings:

Tending Bearing Images

Outer Ring Outside Diameter Photo 1

5.3.3.2 - Fretting corrosion - Minor

Outer Ring Outside Diameter Photo 2

Normal -

Tending Bearing Images

Outer Ring Raceway Photo 1

5.3.3.3 - False brinelling - Minor

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Outer Ring Raceway Photo 2

5.3.3.3 - False brinelling - Minor

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Tending Bearing Images

Inner Ring Raceway Photo 1

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Inner Ring Raceway Photo 2

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Tending Bearing Images

Inner Ring Bore Photo 1

5.3.3.2 - Fretting corrosion - Minor

Inner Ring Bore Photo 2

5.3.3.2 - Fretting corrosion - Minor

Tending Bearing Images

Rolling Elements Photo 1

5.3.3.3 - False brinelling - Minor

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Rolling Elements Photo 2

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Outer Ring Outside Diameter (OD)Normal

Outer Ring Raceway (ORR)5.3.3.3 - False brinelling - Minor5.2.2 - Abrasive wear - Minor5.5.3 - Indentation from debris - Minor

Inner Ring Raceway (IRR)5.2.2 - Abrasive wear - Minor5.5.3 - Indentation from debris - Minor

Lubrication: oil

Inner Ring Bore5.3.3.2 - Fretting corrosion -

Rolling Elements5.2.2 - Abrasive wear - Minor5.5.3 - Indentation from debris - Minor

CageNormal

Drive Bearing Inspection

Sofidel America DCT 100 HS 2522 Suction Press Roll

Recommendations: Reuse Bearing Remanufacture Bearing Replace Bearing

Bearing can be reused and (should/will) be thoroughly cleaned, coated with anti-corrosive material,and protected during storage prior to re-installation on journal bearing seat, per SKF.

Bearing Nomenclature: Inner Race Rotation Outer Race Rotation

FAG 239/630.BK.MB.C3.T52BW

Comments:

Lightly hand scotchbright false brinelling marks, fully clean, and reuse with current ORR load zonerelocated. Also review housing & bearing cleanliness during overhauling, housing sealing design, oilfiltration, roll storage, and roll transit techniques. Contact SKF for further assistance.

Inspection Findings:

Drive Bearing Images

Outer Ring Outside Diameter Photo 1

Normal -

Outer Ring Outside Diameter Photo 2

Normal -

Drive Bearing Images

Outer Ring Raceway Photo 1

5.3.3.3 - False brinelling - Minor

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Outer Ring Raceway Photo 2

5.3.3.3 - False brinelling - Minor

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Drive Bearing Images

Inner Ring Raceway Photo 1

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Inner Ring Raceway Photo 2

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Drive Bearing Images

Inner Ring Bore Photo 1

5.3.3.2 - Fretting corrosion -

Inner Ring Bore Photo 2

5.3.3.2 - Fretting corrosion -

Drive Bearing Images

Rolling Elements Photo 1

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor

Rolling Elements Photo 2

5.2.2 - Abrasive wear - Minor

5.5.3 - Indentation from debris - Minor