![Page 1: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/1.jpg)
Adam Kueltzo# & Julie Lam*
Thornton Fractional North High School #
and Maine East High School *
August 2, 2007
University of Illinois at ChicagoAdvanced Materials Research Laboratory (AMReL)
Mentors: Dr. G. Jursich and Dr. C.G. Takoudis
Atomic Layer Deposition of Novel High Dielectric Constant Materials
![Page 2: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/2.jpg)
Motivation for ResearchTo work with new high dielectric constant (k) materials such as and HfO2 and Y2O3 to replace SiO2 in semiconductors
To run experiments on the atomic layer deposition (ALD) reactor to examine thin film growth rate
To analyze the resulting thin films on silicon using spectral ellipsometry, Fourier Transform Infrared (FTIR) spectroscopy and X-ray Photoelectron Spectroscopy (XPS)
![Page 3: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/3.jpg)
HypothesesA self-limiting reaction between an yttrium precursor, an oxidizer, and the silicon substrate
Good film uniformity on the substrate (using a spectral ellipsometer)
Absence of organic compounds in the resulting film structures (using FTIR spectroscopy)
Stoichiometry of the high-k material and the bonding states of the elements (using XP Spectroscopy)
![Page 4: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/4.jpg)
Moore’s LawAccording to Moore’s Law, the number of transistors per microprocessor should double every two years
www.intel.com/technology/mooreslaw/index.htm
![Page 5: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/5.jpg)
CapacitanceEquation for capacitance:
C = k ε0 At
C = capacitancek = dielectric constantε0 = permittivity of free space
in vacuumA = area t = thickness
www.dvhardware.net/news/inter_higk-k_metal_gate_transistor.jpg
![Page 6: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/6.jpg)
New High-k Dielectric MaterialsWe are currently working with hafnium oxide and yttrium oxide to produce a dielectric layer gate oxide of ~ 45 nm
Hafnium oxide has a k value of 20-25
Yttrium oxide has a k value of 15-18
![Page 7: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/7.jpg)
Atomic Layer Deposition (ALD)Uses pulses of gaseous reactants (precursor and oxidizer) alternately fed into the reactor
Produces one atomic layer at a time on substrates
Film thickness depends on number of deposition cycles
www.icknowledge.com/misc_technology/Atomic%20Layer%20Deposition%www.icknowledge.com/misc_technology/Atomic%20Layer%20Deposition%20Briefing.pdf20Briefing.pdf
yttrium
hafnium
reactor
H2O
![Page 8: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/8.jpg)
ALD Process“One Cycle”PrecursorPurge (N2)Oxidizer (H2O)Purge (N2)
http://www.cambridgenanotech.com/
![Page 9: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/9.jpg)
Acceptable Temperature WindowALD reactions usually occur between 200-400 °C in the reactor
Above 400 °C, the chemical bonds are not stable and the precursor may decompose
Below 200 °C, the reaction rate is reduced
www.icknowledge.com/misc_technology/Atomic%20Layer%20Deposition%www.icknowledge.com/misc_technology/Atomic%20Layer%20Deposition%20Briefing.pdf20Briefing.pdf
200°C 400°C
![Page 10: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/10.jpg)
Experimental ConditionsALD Reactor
- Downstream: 170 °C- Precursor 2: 140 °C- Precursor 2 Leg: 175 °C- Reactor: 302 °C
yttrium
hafnium
reactordownstreamleg
H2O
![Page 11: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/11.jpg)
Y2O3 Growth Rate vs. Precursor Dosage
140 °C
100 °C
![Page 12: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/12.jpg)
12
3 S1
S2
S3
0
6
12
18
24
30
36
42
48
54
60
Film Thickness (A)
Horizontal
Vertical
Y2O3 Film Uniformity
Silicon WaferP-type
Boron doped(100)
![Page 13: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/13.jpg)
FTIR of Y2O3 on Silicon
-0.01
0
0.01
0.02
0.03
0.04
0.05
700120017002200270032003700
Wavenumber (cm-1)
Abs
orba
nce
(A.U
.)
O-H O-H
Si-OY-O
![Page 14: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/14.jpg)
O 1s
Si 2p
Y 3d
Y 3p
Y 3s
Binding Energy (eV)
Inte
nsity
(arb
. uni
ts)
Survey XP Spectrum of Y2O3 on Si
![Page 15: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/15.jpg)
Si
SiO2
Binding Energy (eV)
Inte
nsity
(arb
. uni
ts)
XP Spectra of Y2O3 on Si As-deposited and after 5 min annealing
![Page 16: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/16.jpg)
Quantification Results
Y Atomic Concentration %: 39.2O Atomic Concentration %: 60.8
O:Y = 60.8/39.2 = 1.5
Therefore Y2O3 was produced on the substrate.
![Page 17: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/17.jpg)
Future WorkTo better define the ALD process conditions
Using two precursors to create thin films with alternating atomic monolayers of HfO2 and Y2O3
![Page 18: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/18.jpg)
What Can We Bring Back?Go more in depth into the scientific method
Not every lab is a cookie cutter
Develop better critical thinking skills
![Page 19: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/19.jpg)
ReferencesAnthony, J.M., Wallace, R.M., & Wilk, G.D. (2001). High-k Gate Dielectrics: Current Status and Materials
Properties Considerations. Applied Physics Review, 89 , 5243-5275.
Brain, Marshall. (n.d.). How Semiconductors Work. [WWW page]. http://computer.howstuffworks.com/diode.htm.
Cambridge NanoTech, Inc. (2003-2007). Cambridge NanoTech: Atomic Layer Deposition Systems. [WWWpage]. http://www.cambridgenanotech.com/.
IC Knowledge LLC. (2004). Technology Backgrounder: Atomic Layer Deposition. [WWWpage]. http://www.icknowledge.com/misc_technology/Atomic%20Layer%20Deposition%20Briefing.pdf.
Intel® Education. (n.d.) Inside The Intel® Manufacturing Process: How Transistors Work. [WWWpage].http://www.intel.com/education/transworks/index.htm.
Mutschler, Ann Steffora. (2007). Intel, IBM Embrace High-k Gates for 45nm. Electronic News.
Peters, Laura. (2007). Behind the Breakdown of High-k Dielectrics.Semiconductor International. p. 30.
Zant, P. V. (2000). Microchip Fabrication (4th ed.). New York: McGraw Hill.
![Page 20: Atomic Layer Deposition of Novel High Dielectric Constant ... · Atomic Layer Deposition of Novel High Dielectric Constant Materials. Motivation for Research yTo work with new high](https://reader034.vdocuments.net/reader034/viewer/2022042708/5f3b4f50745ddf2c063efc00/html5/thumbnails/20.jpg)
Acknowledgements National Science Foundation CMS 0731734 and NSF EEC 0703958
Chicago Science Teacher Research (CSTR) program director: Dr. Andreas Linninger
Mentors: Dr. Greg Jursich and Dr. Christos Takoudis
Doctoral students: Prodyut Majumder and Manish Singh
Program coordinator: Kedar Kulkarni