non-destructive testing in civil · pdf filebam viii.2 mindot 2010 28 bridge investigations...
TRANSCRIPT
![Page 1: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/1.jpg)
1BAM VIII.2 MinDOT 2010
Non-Destructive Testing in Civil Engineering
Herbert WiggenhauserBAM- Federal Institute for Materials Research and Testing
Berlin, Germany
![Page 2: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/2.jpg)
5BAM VIII.2 MinDOT 2010
Bridge Testing
In Germany according to DIN 1076• Regular inspection 3 y • In depth inspection 3 y
after Regular inspection• Special inspection
(e.g. after accident orclimatic hazard)
NDT:• Special Inspection• Procedure
![Page 3: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/3.jpg)
6BAM VIII.2 MinDOT 2010
UngroutedTendon Ducts
Bridge Damages
Not uncommonproblem in bridges built1960-80
![Page 4: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/4.jpg)
7BAM VIII.2 MinDOT 2010
Non-Destructive Testing Problems • Measuring the thickness and geometry• Tendon ducts
• Position• Concrete cover • Grouting• Honeycombs (around them)• Corrosion of strands• Cracks and fissures in strands
• Concerte• Reinforcement (position, cover, diameter)• Localisation of honeycombs• Delaminations• Cracks (position, depth)
• Quality assurance of construction• ….
![Page 5: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/5.jpg)
8BAM VIII.2 MinDOT 2010
The Methods
![Page 6: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/6.jpg)
9BAM VIII.2 MinDOT 2010
Impulse Echo Principle(1) Electro-Magnetic Method Radar
Reflections at interfaces of materials with different dielectric propertiesAntenna of 900 MHz and 1.5 GHz Position of antennas
Radar gram with hyperbola
![Page 7: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/7.jpg)
10BAM VIII.2 MinDOT 2010
(2) Acoustic Methods Ultrasonic Echo/ Impact-Echo
Ultrasonic Measurement Device Impact-Echo Measurement Device
Reflections at interfaces of materials with different acoustical properties
Shear waves
center frequency of 50 kHz
Measurement head
24 point-contact transducers
without coupling agent
Frequency range
from 1Hz to 40 kHz
Frequency spectrum analysis
multiple reflections(recorded in the time domain)
![Page 8: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/8.jpg)
11BAM VIII.2 MinDOT 2010
Automation and Scanning
![Page 9: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/9.jpg)
12BAM VIII.2 MinDOT 2010
Scanner Systems
1.6 m x 1.6 m
4 m x 10 m
Scanning Area Speed:
Ultrasonic Echo/Impact Echo1m2/h, 0.02 m point grid
Radar15m2/h, 0.05 m line grid
1.6 m x 10 m
1.2 m x 1.6 m
![Page 10: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/10.jpg)
Multipurpose Scanner System mounted on LCS
Ultrasonic- / Impact-Echo
(Combined sensor head) Radar (1.5 GHz antenna)
13BAM IV.4
Scanner Systems
![Page 11: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/11.jpg)
14BAM VIII.2 MinDOT 2010
Scanner Systems
![Page 12: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/12.jpg)
15BAM VIII.2 MinDOT 2010
► Small leightweightscanner with vaccuumattachement
► Two ultrasound sensors (dry coupled) to reducemeasurement time
Scanner Systems
![Page 13: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/13.jpg)
16BAM VIII.2 MinDOT 2010
Data Fusion and Visualization
![Page 14: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/14.jpg)
17BAM VIII.2 MinDOT 2010
Location of tendon ductsand voids
Reinforced concrete slab
3-D imaging of the results
a
a
Section a-a without reconstruction calculation
Section a-a with reconstruction calculation
reinforcement
reinforcement
void tendon duct
Radar – Data fusion and imaging
![Page 15: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/15.jpg)
18BAM VIII.2 MinDOT 2010
2-dimensional measurement on the surface of structures
B-Scan
plots perpendicular to the measurement surface (x-y plane)
C-Scan
plots parallel to the measurement surface (x-y plane)
Projections and Animations of consecutive scans
3D-Reconstruction
Data Fusion
Focusing of reflected signals using SAFT(Synthetic Aperture Focusing Technique)
Superposition of data
Surface
![Page 16: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/16.jpg)
19BAM VIII.2 MinDOT 2010
Validation
![Page 17: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/17.jpg)
20BAM VIII.2 MinDOT 2010
Large Large ConcreteConcrete SlabSlab (LCS) at BAM (LCS) at BAM
11 Tendon ducts with strands (length 4 m, diameter 40 … 100 mm)Grouting defects, Grouting by DSI
1. Section - Tendon ducts
Facility for various tests and measurements for the improvement of NDT-CE methods
Reference specimen for comparisonof different methods (=>validation)
Validation
![Page 18: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/18.jpg)
21BAM VIII.2 MinDOT 2010
2. Section - Voids and auxiliary devicesVoids:
Compaction faults (gravel pockets)
Auxiliary elements:
Inlet for water and salt-solution through a tube from the bottom side into high porosity structure
Thermoelements (for Thermography)
Stainless steel-plate for backside reflection calibration
Plastic tubes (for Radiography)
Honeycombs
Thermoelements
Steel-plate
Plastic tubes
Water inlet
Validation
![Page 19: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/19.jpg)
22BAM VIII.2 MinDOT 2010
Impact-Echo: Imaging of apparent thickness of slab (C-scan)
Indirect indication of grouting defects
Y-position/mm
X-p
ositi
on/m
m
Validation
![Page 20: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/20.jpg)
23BAM VIII.2 MinDOT 2010
ImpactImpact--Echo: Echo: D-Scan across DuctsFr
eque
ncy/
kHz
X-position/mm
Shifting of back wall echo caused by the tendon ducts
Validation
![Page 21: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/21.jpg)
RawRaw datadata of GBP (3D)of GBP (3D)
X-Position in cm
Y-P
ositi
on in
cm
9600
375
24BAM IV.4
Validation
![Page 22: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/22.jpg)
rebars
reduced depths
ducts
RADAR:RADAR: RawRaw radargramradargram of a of a longlong tracetrace
Dep
th in
mm
Tran
sit t
ime
in n
s
25BAM IV.4
Validation
![Page 23: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/23.jpg)
RawRaw CC--scanscan ((depthdepth sliceslice) at a ) at a depthdepth of 10 cmof 10 cm
0 X-Position in cm
Y-P
ositi
on in
cm
9600
375
ductcorrosion mat
26BAM IV.4
Validation
![Page 24: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/24.jpg)
27BAM VIII.2 MinDOT 2010
Bridge Examples
![Page 25: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/25.jpg)
28BAM VIII.2 MinDOT 2010
Bridge investigations applying NDTBridge investigations applying NDT--CECEBridge deck: Full field investigation 8 Measuring field for detailed investigation with Radar, Ultrasonic echo, impact-echo, (magnetic stray field) (1999)
Girder and Bridge deck:Scanning Echo methods fortendon ducts and honeycombing (2001)
New: Large field investigation with automated scanning system for echomethods (2003)
![Page 26: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/26.jpg)
29BAM VIII.2 MinDOT 2010
Application at postApplication at post--tensioned concrete bridgetensioned concrete bridgeLarge Area Investigation (Scanner)Large Area Investigation (Scanner)
• Radar• Impact-Echo• Ultrasonic Echo
ConstructionCantilever unicellular box bridge Length: 480 m Prestressed in longitudinal and transversal direction Constructed 1966, deconstruction 2004
See: P. HaardtThM-I
![Page 27: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/27.jpg)
30BAM VIII.2 MinDOT 2010
ResultsMeasurements on a post-tensioned bridge deck
Test Area on the top: 4.0 m x 10.0 mTest Area on the bottom: 3.0 m x 10.0 m
tendon ducts with diameters of 45 mm, each with 6 wires
thickness of the deck 23 - 38 cm
![Page 28: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/28.jpg)
31BAM VIII.2 MinDOT 2010
Radar – Datafusion
Bridge deck: of radar data from the top side and bottom side Superposition (Polarization in x- und y-direction, maximum of magnitude is represented)Movie of slices parallel to the surface:
![Page 29: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/29.jpg)
32BAM VIII.2 MinDOT 2010
2 Data Sets
recorded with the 1.5 GHz-antenna
with polarization in x and y-direction
3D-Reconstruction with SAFT
(Synthetic Aperture Focusing Technique)
Data FusionTest Area 4.0 m x 10.0 m
Radar-Visualization of the Results as 3D-Animation
![Page 30: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/30.jpg)
33BAM VIII.2 MinDOT 2010
B-Projection(for a certain y-range)
D-Projection(perpendicular to the bridge axis)
20 kHz
9 kHz
2 kHz20
kH
z
9 kH
z
2 kH
z
Duct investigation (Impact-Echo)
Thic
knes
s
Bridge deck top side: C-Projection close behind the back wall
![Page 31: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/31.jpg)
34BAM VIII.2 MinDOT 2010
Right:C-scan depth about 8 cm
step width 5 cm
Left: SAFT-C-Projection depth 11,7 cm … 12,1 cmstep width 2,5 cm
Ultrasound: Duct investigation
Highreflectionintensity atboth sides
Bridge deck bottom side
![Page 32: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/32.jpg)
35BAM VIII.2 MinDOT 2010
Bridge-deck: Destructiv testing: 35 cores, endoscopy
Box girder wall (longitudinal tendon ducts)
Bridge deck (transverse tendon ducts): Very good grouting condition
VerificationVerification
![Page 33: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/33.jpg)
36BAM VIII.2 MinDOT 2010
Measurements on webs of box girder bridges
Test Area: 10 m (length) x 1.5 m (height)
thickness of the web 50 cm (83 cm in the area of anchoring of the pre-stressing)
bridge under unaffected traffic
simultaneous mounting of the impact-echo and ultrasonic sensors on the scanner
![Page 34: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/34.jpg)
37BAM VIII.2 MinDOT 2010
Data Fusion of Radar and Ultrasonic Echo
Animated sections parallel to the surface through the measurement depths from 0 cm to 60 cm
3D-reconstructed and fused radar data sets (1.5 GHz-antenna)and
3D-reconstructed ultrasonic echo data set
![Page 35: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/35.jpg)
38BAM VIII.2 MinDOT 2010
Coupling area
Radar
SAFT-C-Scan parallel to the surface in a measurement depth of 7.5 cm
![Page 36: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/36.jpg)
39BAM VIII.2 MinDOT 2010
Ultrasonic Echo
SAFT-C-Projection parallel to the measurement surface at the range of depth from 22 cm to 28 cm
Coupling area
![Page 37: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/37.jpg)
40BAM VIII.2 MinDOT 2010
Ultrasonic Echo
Dep
th y
in c
m
600 4020 Height z in cm
6020
150
100
Box girder web Thickness: 50 cm Height of test area: 1.40 m
SAFT-B-Scan
Inside of the web
Test
are
a
Box girder web Thickness: 75 cm Height of test area: 1.60 m
SAFT-B-Projection Depth of test area: 1.20 m
Outside of the web
Height z in cm
Depth y in cm
![Page 38: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/38.jpg)
41BAM VIII.2 MinDOT 2010
Test Area on the bottom side of the deck, 0.96 m x 18.40 m:
ultrasonic echo measurements were done in 23 scanning areas length of 2 m x 0.40 m
Measurements on a bridge deck, pre-stressed in longitudinal direction
![Page 39: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/39.jpg)
42BAM VIII.2 MinDOT 2010
Ultrasonic Echo
Tendon duct 4
Tendon duct 2
Tendon duct 3
Tendon duct 1 x in mm
SAFT-C-Projection in the depth range of z = 200 – 400 mm
Right: SAFT-B-Projection about the whole length of 18.40 m
![Page 40: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/40.jpg)
43BAM VIII.2 MinDOT 2010
Evaluation of the Intensity of Ultrasonic Echo-Signals
Back wall of the structure in a depth of 1.75 m
Tendon ductReinforcement bars
04008001840
500
1500
Length x in mm
Dep
th z
in m
m
12001600
SAFT-B-Projection about the range with the tendon duct 2
![Page 41: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/41.jpg)
44BAM VIII.2 MinDOT 2010
Transmitted pulse Reflected pulse
Pulse Behaviour of Ultrasonic Echo-Signals
Reflections on steel in concrete
No transfers of phase
Reflection on air-inclusions in concrete
Transfer of phase
![Page 42: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/42.jpg)
45BAM VIII.2 MinDOT 2010
Reflection on the back wall of the structures
(topside in a depth of 1.75 m) :transfer of phase (red-green-red)
Length x in mm
Dep
thz
i n m
m
Reflection on the upper side of a tendon duct:no transfer of phase (green-red-green)
Dep
t hz
i n m
m
Length x in mm
SAFT-B-Projection (Phase)
Top: about y=1940-2100 mm, Down: about y=1828-1926 mm (tendon duct 2)
Evaluation of Pulse Behaviour of Ultrasonic Echo-Signals
![Page 43: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/43.jpg)
46BAM VIII.2 MinDOT 2010
Scheel, Hillemeier, TUBFlohrer, HochTief
Locating tendon cracks in PT Concrete
![Page 44: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/44.jpg)
47BAM VIII.2 MinDOT 2010
Conclusions
![Page 45: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/45.jpg)
48BAM VIII.2 MinDOT 2010
Localization, Concrete Coverreinforcing rebars, tendon ducts
Condition of tendon ducts
Verification43 cores, endoscopy
RADAR:Fast accurate 3D-imaging (Visualization) • Measuring with high precisionImpact-echo: Large area imaging
and back wall echo shiftUltrasonic echo: Direct imaging• No clear indication of grouting faultsConfirmation: No grouting fault
Successful application at a postSuccessful application at a post--tensioned concrete bridge:tensioned concrete bridge:
ConclusionConclusionAutomated Measuring system (scanner):Automated Measuring system (scanner): Successful application at large concrete slab (LCS) and on bridges• LCS is very well suited for comparison of test methods• RADAR can localize tendons with high accuracy• Ultrasonic echo (dry contact) can localize ducts and identify grouting defects
• Impact-echo gives indirect indication of grouting defects
![Page 46: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/46.jpg)
49BAM VIII.2 MinDOT 2010
What‘s next?
![Page 47: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/47.jpg)
50BAM VIII.2 MinDOT 2010
• Crack documentation on Metropolitan (1995) Highways Tokyo (View area 2 x 2 m2)
Laser
Robot
![Page 48: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/48.jpg)
51BAM VIII.2 MinDOT 2010
Robot
Self navigating Robot for horizontal surfaces (Park decks)
Video on YouTube: BestoScan
![Page 49: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/49.jpg)
52BAM VIII.2 MinDOT 2010
Robot: Possible sensors
![Page 50: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/50.jpg)
53BAM VIII.2 MinDOT 2010
Development of the On-Site SCAnneR (OSSCAR)
Requirements:Robust, transportable,on-site results,controller, data collection,data analysis and presentation in one software
Consortium: Integrated project OSSCARfounded by BMWi, Coordinator: BAM
![Page 51: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/51.jpg)
54BAM VIII.2 MinDOT 2010
Method combination in OSSCARSynergy by combination of radar, ultrasonic echo and eddy current
Eddy currentRadar Ultrasonic echo
Suitable for metallic reflectors
Limited penetration depth (young concrete)
Larger penetration depth also in areas with high reinforcement ratio
Limited resolution of single rebars
Measurement of reinforcement diameter
Information only about upper layer
Calibration of radar (ε: dielectric constant)
![Page 52: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/52.jpg)
56BAM VIII.2 MinDOT 2010
First on-site applicationBridge close to Frankfurt over the river Main (2009-Sep)
![Page 53: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/53.jpg)
58BAM VIII.2 MinDOT 2010
• Climbing machine equipped with • camera• radar• impact-echo• ...
ROSY climbing machine (Yberle)
Robot
![Page 54: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/54.jpg)
59BAM VIII.2 MinDOT 2010
Robot
EC Project: Robosense
![Page 55: Non-Destructive Testing in Civil · PDF fileBAM VIII.2 MinDOT 2010 28 Bridge investigations applying NDT-CE Bridge deck: Full field investigation 8 Measuring field for detailed investigation](https://reader036.vdocuments.net/reader036/viewer/2022070606/5a7034547f8b9a93538bc332/html5/thumbnails/55.jpg)
60BAM VIII.2 MinDOT 2010
ASV Fulda
Vienna City Administration
Research groupsupported by the DFG (Deutsche Forschungsgemeinschaft)
BAM
Thank you for attention !